From Physical Scanning to Casting Simulation: Identifying Filling and Shrinkage Risks in a Housing
Published:
2026-11-03
The 3D model of aluminum alloy differential cover was reconstructed, and ProCAST was used to analyze filling, solidification and defect prediction.
Differential cover after sandblasting for 3D scanning, Figure 1 of the original paper (CC BY 4.0)
Geometry Reconstruction, Process Conditions and Numerical Methods
When there are 0 parts to redesign the casting plan, the physical scan can provide the geometric basis, but the complete casting model also needs to deal with machining allowance, runner, overflow and equipment boundary. Taking an automobile differential cover as an example, the study connected optical 3D scanning, reverse engineering and numerical simulation in series to check for possible filling and solidification problems before manufacturing production molds. This case uses high pressure die casting of aluminum alloy, and the temperature of molten metal, injection motion and metal mold conditions in this paper correspond to this process.
The original was approximately 206 × 104 × 79 mm in shape and measured to have a mass of 1.09 kg. Sand blasting prior to scanning to remove surface contamination, oxide and residue improves optical measurement conditions. The ATOS 5X scanner uses structured blue light to acquire surface point clouds. Reference points were set around 0 to locate the relative position between 0 and each scan. Complex surfaces and occlusions make it difficult to achieve full geometry with a single fixture, so a second fixture position and rotating fixture are also used to gradually supplement the differently oriented surfaces.
FIGS. 2 and 3 show the measurement arrangement and the merged polygon model. GOM Inspect 2021 is used for point cloud alignment, noise cleaning, and mesh processing. Openings, occlusions, and incomplete surfaces that cannot be directly measured are completed based on adjacent structures, and the mesh is closed to a shape that can be used for subsequent modeling. This step determines whether the model can be numerically calculated and also requires engineers to distinguish between areas measured by the original and areas reconstructed.
Solid models are then built in SolidWorks 2020, simplifying details that have less impact on casting analysis and adding allowances for subsequent machining. Figure 4 specifically illustrates the adjustment of the threaded bottom hole. The size of the finished hole come from machining, and the casting blank leaves material, so it is not possible to treat all size of the finished appearance as the as-cast geometry. After completing the blank model, the author arranges the runner and overflow elements to form the system of Figure 6.
The ProCAST 2023.0 model further incorporates a metal die, press chamber, and punch. The computational mesh contains approximately 149,000 two-dimensional elements and 2,699,000 three-dimensional elements. Local refinement in the casting region balances detail resolution against computational cost. The grid not only includes 0 pieces, but also covers the parts in contact with liquid metal and heat transfer. The spatial relationship, material and boundary conditions of the model jointly determine the subsequent velocity field, temperature field and solidification analysis.
Table 1 AlSi9Cu3 aluminum alloy is used, the liquidus line given by the material library is about 586 ℃, the solidus line is about 510 ℃, and the initial molten metal temperature is set at 680 ℃. H13 tool steel was used for the mould, and the initial temperature was 210 ℃. The punch material is beryllium copper and the initial temperature is 80 ℃. The thermal conductivity of the alloy is approximately 140 W/m/Kelvin at room temperature and 85 W/m/Kelvin at casting temperature. The surface of the mold is provided with a water-based coating with a nominal thickness of 100 microns, and the interfacial heat transfer coefficient is specified according to the original Table 2.
The model does not explicitly establish additional mold cooling circuits, and the external cooling medium is set to 20 ° C air. This means that the simulated temperature field corresponds to the defined simplified heat transfer environment. If there is another waterway or spray cooling on site, it is necessary to reset the corresponding thermal boundary, and the result cannot be used only by replacing the material name. The authors also list material library data together with actual equipment settings so that model conditions can be traced.
The ram displacement and velocity of Figure 9 are divided into three intervals. From zero to 320 mm in the front section, the speed gradually increased to 0.4 meters per second; The rapid injection range is from 320 to 430 mm, and the speed is increased to 3.5 meters per second; In the last ten millimeters, the velocity drops to 2.5 meters per second. The last segment represents the ram motion associated with the pressurization phase, and the model does not directly specify an independent pressure curve. Therefore, the analysis should be based on the actual input of displacement and velocity conditions to understand the filling.
The conservation of mass, momentum and energy is used in the calculation. The turbulence is described by the standard turbulent kinetic energy and dissipation rate model. The free surface is tracked by the fluid volume method. The sensible and latent heat of solidification are considered by enthalpy method, and the liquid flow resistance in mushy region is introduced by permeability relation. The specific enthalpy is expressed by the specific heat term of temperature integral and the latent heat term of liquid phase in the formula (7) of the paper. The latent heat released when the solid fraction increases enters the heat equilibrium. These couplings allow the evolution of the filling, temperature drop, and feeding channels to be analyzed in the same calculation.
Filling, Solidification and Predicted Defects
FIGS. 10 and 11 show that a slow phase is set to cause the metal level in the pressure chamber to rise gradually, followed by a fast phase to feed the molten metal into the runner and cavity. There is no obvious violent fluctuation in the model, the overflow part is filled in the later stage, and the cavity is filled before the metal liquid drops to the liquidus line. According to this, the author thinks that this scheme has better filling conditions, but the actual porosity, cold shut and under-pouring still need to be checked by product inspection.
The solid phase distribution in Fig. 12 shows that the solidification is late in the local thickness such as the reinforced area around the hole and the larger rib plate. These areas store more heat, and after the surrounding thin walls solidify first, the liquid supply path may gradually narrow. Figure 13 evaluates solidification time over the temperature interval of approximately 586.6–510.6 ℃. Values at different positions in the casting range from approximately 1.85 to 8.80 s. Spatial differences are more indicative of the location of risk than individual total times, as the precedence of the last solidified thickness over the surrounding area determines whether feeding can continue.
Figure 14 shows the entrainment index, with higher values concentrated near the final filling position and some cooling ribs, and values in the analysis area ranging from about 0.0004 to 0.002 g/cm3. This is an estimate of the entrainment output by the software. The original text clearly does not give an independent acceptance threshold, nor does it provide a calibration relationship between the actual casting porosity and this index. It can be used to arrange exhaust improvement and focus on inspection positions, and the value itself cannot be used as a product porosity acceptance criterion.
FIG. 15 shows shrinkage defect prediction from different perspectives and cross-sections. A local maximum of approximately 80 percent occurs around the upper mounting hole. The authors consider this area to be the most in need of further investigation, since variations in wall thickness and solidification order of adjacent structures may interrupt the feeding. This value corresponds to the local prediction output of the model, and the actual pore content needs to be detected. Taking the local maximum value as the scrap rate of the whole cover will change the meaning of the original result.
There are also areas of concern near overflow elements. The position is favorable for receiving the liquid metal and air after arrival, but the local late solidification may cause shrinkage risk in the upstream part. The original paper therefore discussed runner, overflow, and thick-walled geometries simultaneously, without equating increasing overflow directly with eliminating defects. It is necessary to judge how the modification will affect the liquid supply and exhaust according to the flow direction and solidification time diagram, and then compare the old and new schemes.
The authors did not perform quantitative verification of defects after trial casting of production molds, nor did they report the reduction of defective rate confirmed by inspection in Group 1. The results retained in this paper are derived from numerical calculations under the assumed boundary conditions. The useful outcome of the study is to identify which positions should be adjusted or inspected first, and what information needs to be completed from scan to blank model, process system and simulation. The predicted hot spots can be checked with the test results of real castings, so that the interpretation ability of this model to the field can be further evaluated.
For other castings, it is possible to obtain reliable geometry first, then complete the difference between as-cast and machined state, and then incorporate equipment, materials and heat transfer conditions into the working sequence of the same model. The ceramic shell, gravity filling and feeding mode of investment casting need to be defined independently, and the injection speed of this case cannot be copied. Clarifying the scope of the process and the source of the results helps to distinguish between methods that can be used for reference and specific settings that need to be retested during technical exchanges.
Karlo Jurković、Tomislav Staroveški、Branko Bauer、Tomislav Gotić,Materials,2026,19(21),4675。 DOI 10.3390/ma19214675。 According to the original paper arrangement, with pictures quoted from the original paper.Download PDF · Original Paper · CC BY 4.0