Reducing Bubbles in Silicone-Rubber Molds for Investment-Casting Wax Patterns


Published: 

2026-08-25

The bubble, surface state and curing time of silicone rubber mold vulcanized at room temperature were evaluated by comparing 18 sets of stirring speed and ratio.

Effect of ratio and rotational speed on catalyst dispersion, Figure 2 (CC BY 4.0)

Effect of ratio and rotational speed on catalyst dispersion, Figure 2 (CC BY 4.0)

Mixing Ratios, Stirring and Quality Assessment

Small batch investment casting can be used to replicate wax patterns with room temperature vulcanized silicone rubber molds. Bubbles, hard lumps or partial uncured on the surface of the mold easily affect the surface and contour of the wax mold, so the dispersion state of silicone rubber and catalyst is regarded as the key observation point. The study used RTV-52 silicone rubber and RTV Blue catalyst with a custom DC-motor stirring apparatus, comparing speeds of 50, 100 and 200 r/min.

The volume ratio of silicone rubber and catalyst was adopted, and 6 grades were adopted from 35∶1 to 40∶1, and 18 groups of conditions were formed with 3 grades of rotation speed. 54 samples were prepared by mixing, stirring, pouring and curing 3 times independently for each group. Stir for about 6 - 10 minutes, then pour the mixture into a cylindrical trial mold 7.5 cm in diameter and 5 cm in height and cure at room temperature. Figure 1 shows the test flow from withdrawal to wax pattern application.

The extent of catalyst dispersion was estimated by the visual uniformity of blue in the sample. The surface state was graded as rough, smoother and smoother, and the bubbles were graded as none, less and more, and the occurrence of catalyst lumps or local hardening was observed. From the time of completion of mixing until the sample can be taken and placed without visible deformation. Table 3 summarizes the three independent tests, with cure times expressed as mean and standard deviation.

Each iteration starts with separate measurements of silica gel and catalyst, which are then mixed and poured separately, so three iterations reflect fluctuations in the entire operation. The author points out that measurement deviation, stirring time, room temperature, pouring conditions and manual judgment of end point may cause differences. The practical criterion of no visible deformation during picking and placing is adopted for curing end point. This criterion facilitates comparison of turnaround times between groups, and the study did not use instrumentation to determine the point at which chemical crosslinking was complete.

The smaller the ratio, the more catalysts the bulk silicone rubber corresponds to. If stirring can only drive the material near the blade, the position of the high viscosity silicone rubber away from the blade may still form a slow flow area. Local color is thick and other positions are light, which means that the catalyst is unevenly distributed in the whole material. The authors use this dispersion deficiency to explain why local hard lumps, surface irregularities and overall slow formation occur simultaneously in some samples. The blue catalyst was used in the test to provide a uniform visual control for the different combinations.

Results of Parameter Combinations and Their Applicability

FIGS. 2 to 4 compare the degree of dispersion with the curing time after changing the rotation speed and the ratio. Under this equipment and material condition, higher rotation speed usually makes the blue catalyst more evenly distributed and shortens the time to reach the accessible state. However, bubbles will not decrease with the increase of speed, and some high speed combinations still have more bubbles. When choosing the formulation, the author compares the surface smoothness, bubbles, agglomeration and curing speed.

When the six ratios are put together at each speed, the average visual dispersion of Figure 4 is 56.7%, 70.0% and 83.3% respectively. Figure 2 shows that the estimate for the 50 r/min group is 40%{70%, with 100 r/min increasing to 60%{80%, and 200 r/min to 70%{90%. In Fig. 3, the curing-time ranges for the three stirring speeds are approximately 18 h to over 24 h, 6–20 h, and 2–6 h, respectively. After the speed is increased, there are still differences between the ratios, so when reading these three diagrams, the comparison of the same ratio across the speed should be combined with the comparison of the ratios at the same speed.

At a fixed ratio of 38:1, see Table 3, that dispersion was about 70% visually at 50 r/min, and the cure time was about 18 hours, which was generally poor. At 100 r/min, it was about 80% and 6 hours, and the comprehensive observation was general. No visible bubbles were recorded in both groups. At 200 r/min, dispersion is estimated to increase to about 90%, curing takes about 2 hours, the surface is smooth, and the bubble level is low. This comparison shows that low rpm is selected for visible bubbles alone, but mix and rpm need to be selected together considering cure turnaround and mold surface.

Then fix 200 r/min to see the ratio. The cure times of 35:1, 36:1, and 37:1 were approximately 2.5, 2, and 2 hours, respectively, and were all recorded as bubbly. The dispersion estimates for 39:1 and 40:1 were both 90%, with fewer bubbles, but curing took about 5 and 6 hours, respectively. 38:1 shortened the occupation time at similar dispersion level and bubble grade. It is a comprehensive scheme selected by the author from these 18 groups. The visual score of approximately 90% for all 3 groups does not mean that the turnover can be scheduled at the same time.

The discussion section explains these changes in terms of the sequence of flow and solidification. With the increase of rotational speed, the viscous material passes through the mixing zone near the blade more frequently, which helps to reduce the concentration gradient of catalyst. Air may also be introduced when the blades disturb the free surface and the rubber folds inward. As silicone rubber gradually forms a crosslinked network, the fluidity of the compound decreases, and bubbles that have not yet floated to the surface may remain inside or form pits on the surface. The combination with high catalyst proportion solidifies faster, and the time left for some bubbles to float may also be shortened. The paper relates this explanation to the phenomena in Table 3 and makes it clear that vacuum degassing was not used in the test.

It is worth distinguishing between the catalyst dispersion and bubble level observed by the author during the molding stage. The paper did not use instruments to measure silicone rubber viscosity, local shear rate, bubble size distribution, pore volume fraction, or surface roughness. The discussion of compound circulation, bubble rise and crosslinking rate belongs to the explanation of experimental phenomena. Improved mold conditions are expected to reduce surface problems transmitted to the wax pattern, but these data are not enough to quantitatively calculate the size error of the wax pattern or the yield rate of the final metal casting.

The same preparation principle was also applied to wax pattern making of two-piece silicone rubber mold. When the process is changed, the mold stirring conditions, demoulding judgment and wax pattern inspection results can be recorded separately, because the finished surface is also affected by the subsequent wax filling, cooling and exhaust. If vacuum degassing is used in the actual workshop, or the container and blades are replaced, the dispersion and entrainment corresponding to the same speed may also change. Record the material combination, proportion, charge amount and operation time together to judge whether the trial production results are close to the paper conditions.

In small batch or prototype production, the paper compares the use of silicone rubber mold with metal wax mold. Silicone rubber can be directly overmolded from the mother sample. When the design is frequently changed or the quantity is small, the preliminary mold preparation is relatively simple. Metal molds require machining, but have advantages in durability, size stability, and automation under high volume conditions. The cost and turnover advantages mentioned in this article are a discussion of production conditions. The author does not compare the man-hours, energy consumption, life or actual cost per qualified wax pattern of the two molds.

As far as turn-around time is concerned, the paper judges the improvement range from the time when the sample enters the state of taking and releasing. The low speed group required about 1 day for multiple compounding and about 2 hours for selecting conditions, which may reduce the wait between molding and waxing. However, shorter waiting times also mean that the operator needs to finish pouring while the compound is still flowing. The flow path in the container will change after amplification, and the mixing quality of the sample can not be automatically reproduced by maintaining the rotation speed and proportion. It is suggested that demoulding, wax leakage, size accuracy, surface roughness and mold service life should be checked under actual batch conditions, and then whether the process is stable or not should be evaluated.

Subsequent verification can also convert visual observations into repeatable quantitative indicators. In this paper, the viscosity and rheological properties of rubber were measured, the bubble size and distribution were estimated by image analysis, and vacuum deaeration was used as control. To determine whether the improvement in the molding process has actually reduced rework of the wax pattern, it is also necessary to measure the wax pattern surface and size under the same wax pressing and cooling conditions. The mold, wax pattern and final casting are evaluated separately to determine where the effect is verified.

These parameters apply in conjunction with RTV-52, RTV Blue, the specified specimen dimensions and the stirring apparatus. Blend shear, entrained air, and cure rate may vary when silica gel, catalyst, or charge is increased. Small batch trial production can follow the control method in this paper, test step by step under the same set of materials and equipment, and then confirm the process window with the actual forming quality of wax pattern.

Peter Prayogo Pangestu、Martin Andre Setyawan,Angkasa: Jurnal Ilmiah Bidang Teknologi,18(3)。 Original Paper · PDF · CC BY 4.0