Comparing Casting Simulation with Trial Castings of Perforated High-Manganese-Steel Liners


Published: 

2026-06-24

Holes in the porous liner alter the cooling process. The research team incorporated the effect of voids on heat conduction into the simulation, and then used the actual test casting to check the formation, hole location and working surface defects, and compared the model predictions with the casting performance.

Sample of the trial casting, taken from the paper by Ran et al., Fig. 9 (CC BY 4.0)

Fig. 9 Trial casting

Abstract

In the investment casting of ZGMn13Cr2 high manganese steel porous liner, the internal cavity will make the temperature field and defect prediction results obtained by traditional numerical simulation deviate. in this study, that equivalent heat conduction model of Bruggeman porou media is introduced and modify to suit the porous castings. After calculating the overall porosity of the liner casting, the researchers calculated an equivalent thermal conductivity scaling factor of 0.675 for the liner based on the modified Bruggeman model and used this correction factor to simulate the liner in ProCAST software.

The simulation results show that the modified model significantly improves the uniformity of temperature field and synchronization of solidification process, and improves the accuracy of shrinkage cavity prediction. The shrinkage cavity volume at each monitoring point decreased by 44.2%, and the uniformity of defect distribution was improved obviously. Finally, the casting results of lining plate show that the modified model is more consistent with the actual casting in macroscopic forming, hole location accuracy and defect distribution trend. This study provides a new method for process simulation optimization of complex porous structure castings, and practical experience for casting simulation and actual forming of porous products.

keywordZGMn13Cr2, porous media, equivalent thermal conductivity model, investment casting, numerical simulation

Liner Geometry, Gating System and Thermal-Property Corrections

Ran et al. studied a ZGMn13Cr2 high manganese steel porous liner. There are 145 tapered through holes in the liner, which occupy a considerable part of the volume. Simulating solidification, how the metal and cavity around the hole conduct heat affects the software's ability to determine which parts cool down first and which parts still need liquid metal feeding. The researchers calculated the solid and void volumes of the liner separately, yielding an overall porosity of about 23 percent. The calculation here is the proportion of existing through holes in the design, and the shrinkage cavity generated in the casting process is separately counted.

The 0 pieces shown in Figure 1 of this paper are used for electrolytic aluminum electrolyte self-grinding equipment. The plate thickness is 30 mm, the width is 402 mm, the diameter of the small end of the conical sieve hole is 18 mm, and the diameter of the large end is 27 mm. The filling time is about 14 seconds. According to the minimum flow resistance cross section, the cross section area ratio of sprue, runner and ingate is calculated to be about 1.2∶1.1∶1. The geometric size of sprue is listed in Table 1. the foam pattern and dry sand are use in that trial casting. the term investment cas is used in the discussion of the process, and the actual trial casting proces is clearly written as lost foam casting in section 5.1.

In the heat transfer calculation, the modified Bruggeman equivalent medium model is used to convert the region composed of metal and pores into a continuous medium with equivalent thermal conductivity. According to the simplification of this paper, the contribution of gas conduction is reduced to zero and the radiation term is neglected. With porosity φ and solid-material thermal conductivity kₘ, the ratio of effective thermal conductivity to kₘ is (1−φ)³ᐟ². Substituting φ=0.23 used in the paper gives approximately 0.675. This scale depends on model assumptions and liner geometry. The equivalent values were written into ProCAST material database and compared with the calculation results before and after correction under the same casting scheme.

To assess the resolution of local features such as hole edges, the team compared three global grids of 15, 10, and 5 mm, with subsequent results using a 10 mm grid. Monitoring points are arranged near the center hole and upper, lower, left and right boundary holes, covering the area close to and far from the runner. The two models are compared by temperature history, solidification and cooling results, pore evolution and defect volume distribution in Fig. 4 to Fig. 8.

Shrinkage-Cavity Prediction at Five Points and Casting Validation

After correction, the temperature curves at most monitoring locations are more concentrated, and the time difference between the start of obvious shrinkage cavities everywhere is also reduced. According to Table 2 of the paper, the predicted shrinkage volume of the center hole decreases from 0.240 to 0.157 cm³, the upper boundary decreases from 0.165 to 0.092 cm³, the left boundary decreases from 0.148 to 0.107 cm³, and the right boundary decreases from 0.122 to 0.092 cm³. The lower boundary decreases from 0.121 to 0.108 cm³. After correction, the central hole is still the position with the highest predicted value among the 5 points. The upper boundary decreases by about 44.2%, and the lower boundary decreases by about 10.7%. The difference is explained by the thermal gradient and feeding conditions: the upper region cools earlier, while the lower region is affected by the high temperature metal of the adjacent gating system, and the feeding conditions are different.

To verify these judgments, the research team conducted actual test runs of the center pour scheme. Section 5 of the paper records the process of making foam model, assembling runner, coating refractory layer, filling dry sand and vibrating. The high manganese steel is melted by medium frequency induction furnace, the temperature of molten steel reaches about 1500 ± 10 ℃, and the casting is completed after deoxidation, the whole process is about 14 seconds. Castings are cooled naturally in sand molds and the gating system is removed after sand cleaning.

Figure 9 shows a single liner, a monolithic casting still with a gating system, and a partial face. The author reports that 145 through holes are clearly formed, the hole location and size meet the design requirements, and there is no obvious undercasting or cold gap in the overall outline. Rough grain after sand cleaning can be seen in local working face, and no concentrated macro-shrinkage cavity or crack can be found in the observation range. These physical observations support the corrected predicted defect distribution trends. 44.2% in Table 2 is the simulated predicted value change of the upper boundary hole, and the physical link check is the distribution of formed and visible defects.

Source Jingwei Ran et al., Archives of Foundry Engineering 26(2), 21 - 32. Abstract translated from the original paper, figure 9 quoted from the same text.Original Paper · CC BY 4.0