Reducing Shrinkage Cavities and Foam-Decomposition Surface Defects in Steel Bucket Teeth


Published: 

2026-03-09

A study on lost foam casting of bucket teeth was carried out. The filling speed, feeding channel, foam density and pouring temperature were compared by simulation and trial casting of two sets of pouring and feeding schemes.

Original paper test drawing (CC BY 4.0)

Original paper test drawing (CC BY 4.0)

Defect Locations, Process Conditions and Two Simulated Designs

Excavator teeth withstand mechanical impact and abrasive wear, both material durability, but also need to be assembled with the tooth seat, pin holes and other parts to maintain the appropriate size. The object of study is a bucket tooth made of low alloy steel with a mass of 8.6 kg. The original production process is EPC, and over-center shrinkage cavity and porosity appear. The author chooses to start with the casting feeding system, putting the liquid metal flow, solidification feeding and foam thermal decomposition into the same process analysis, and then using the trial casting to check the surface problems that are not fully presented in the calculation.

The original paper uses L35GSM steel, carbon mass fraction is about 0.32 to 0.4%, manganese is about 1.2 to 1.4%, silicon is about 0.6 to 0.8%, molybdenum is about 0.3 to 0.4%. This case belongs to low alloy steel lost foam casting, the specific pouring temperature and foam treatment conditions and this set of materials and pattern system matching. The useful part of the study lies in the joint diagnosis of the compensation channel and decomposition products.

The expandable polystyrene beads are formed in a mold to obtain a primary foam pattern, and then the runner is bonded and coated with water-based refractory coating. After the coating is dried, the pattern is embedded in dry silica sand and vibrated in a metal flask. Induction crucible furnaces are used for melting, the flask is connected to a vacuum system during pouring, and the residual gas pressure is about 0.04 MPa to help remove foam decomposition products. After the casting is cooled, the runner is removed, and then shot blasting is carried out.

Flow-3D Cast 2023R1 was used to calculate the basic scheme and the improved scheme respectively. The mesh cell size was set to 4 mm, the initial temperature of the molten steel was 1600 C, and the initial temperature of the mold, foam and environment was 20 C. AISI 1040 steel was selected from the material library for approximate research. The author explained that its composition, liquidus and solidus are close to the target material. The two phase transition temperatures are about 1492 ℃ and 1428 ℃ respectively. Material substitution is part of the calculation conditions and affects the interpretation of the temperature field.

The density of the foam model was set at 25.64 kg/m³. The heat transfer coefficients between liquid metal and foam, liquid metal and sand mold, solidified metal and sand mold are 3000, 600 and 200 W/m2/Kelvin respectively. A metal pressure of 6800 Pa is applied to the upper end of the sprue, corresponding to a static pressure height of about 96 mm in the sprue cup. The author fixed these conditions and compared the gating system, so that the calculation results can correspond to the changes caused by different runner layouts.

Figure 1 shows the tooth shape and foam material, Figure 2 records the original process defects, Figure 3 shows the layout of the pattern group in the flask. This sequence provides a practical reference for subsequent defect predictions. Central shrinkage can be checked against simulated hot spots by location of sectioning, and surface cold cuts can be combined with leading edge convergence and foam residue. For a local thin bridge like this above the pin hole, the fact that the entire casting is full does not mean that the two strands of metal form a good connection at the meeting point.

The mold filling of EPC requires continuous replacement of foam with metal, so the calculation cannot simply regard the cavity as the initial cavity. At each time step, the software calculates the amount of heat transferred by the metal to the foam, which in turn estimates the amount of energy consumed by melting, vaporization, and heating, as well as the volume of foam removed, and subtracts this amount of heat from the metal. The metal then enters the corresponding volume of space. This process correlates pattern density, flow front and local cooling.

The defect prediction also records the accumulation of foam decomposition residues at the metal front. When the leading edges meet or bend, residues may be trapped inside the metal, so local concentration peaks are used to locate locations where pinch and joint problems are more likely to occur. It is a model-based risk indicator and cannot be taken directly as physical pore volume. The authors also compared temperature, residue concentration and final shrinkage distribution to distinguish defects from different sources.

Improved Feeding, Trial-Casting Differences and the Final Process

In the calculation of basic scheme, metal enters riser first, and then enters the middle of bucket tooth through ingate. Figure 4 shows flow front velocities of approximately 0.05 to 0.07 m/s; At the end of mold filling, the metal in riser is still hot, but the predicted shrinkage cavity in tooth center is consistent with the actual defect position. Figure 6 further illustrates the presence of a hot spot in the center and the geometry of the ingate connecting the riser to the casting is not conducive to continuous feeding. Risers solidify last and do not automatically ensure that hot spots are always connected to the liquid supply area.

The improved scheme uses larger risers and two short ingates to connect castings. The metal front velocity of Figure 7 drops to 0.03 to 0.05 m/s. The pouring time of the whole group was increased from 10.85 s to 12.68 s, and the weight of the group was adjusted from 31.2 kg to 30.0 kg. The velocity decrease and time extension reflect the filling process after the flow passage is changed. The author also observed that the metal enters from two places and the temperature distribution of castings is more uniform in the improved scheme.

Solidification results in Figures 8 and 9 show that shrinkage cavities are transferred to risers after modification, and the hot energy of the bucket teeth is fed through the ingate. The concentration of foam residue on the surface of most castings decreased, but there was still local concentration near the upper orifice. Therefore, the author also observed whether there was cold shut or under-pouring in these areas during the physical verification. Simulations give directions for improvement while leaving specific locations to be physically inspected.

The surface defects still appeared in some castings when the first round was produced according to the improved system. Tracing revealed that some patterns had a density of 38 to 2040 grams per cubic meter, higher than the 25 to 1030 grams expected by the process. The increase of foam in the same volume changes the amount of heat required to vaporize the molten steel and the burden of decomposition products. The pattern density used in the simulation does not cover these high density patterns, so the original calculation results cannot be used to directly judge these specimens.

The thin bridge above the hole is formed by the confluence of two metal flows, and the calculated temperature is about 1500 ℃. There is both a temperature drop at the front and a possible accumulation of foam residues, and the cold insulation of the physical appearance needs to be explained from both factors. The author adds an overflow point above the hole to provide a destination for metals and residues that arrive last. The tip of the bucket teeth also showed under-pouring in the high-density pattern batch, indicating that only improving center feeding did not cover all mold filling problems.

In order to compensate for the cooling caused by the high density foam, the pouring temperature was increased to 1640 ℃. Although undercasting is reduced, local sand sticking occurs in the group poured earlier from the ladle, so it is not ideal to increase the temperature alone. The final trial casting uses a pattern with a density of 8020 grams per cubic meter, molten steel at 1590 ° C, and increases the overflow above the orifice. Figure 12 of the paper shows the group tree and section, reporting that the tooth body has no center shrinkage and the end face is improved.

The final technological window given by the author includes: adopting improved filling system and overflow position, pattern density controlled from 25 to 1030 g/m3, pouring temperature controlled from 1580 to 1610 ℃. The size and surface of the batch is controlled to meet the pattern requirements, and the protocol is subsequently used for batch production of the bucket tooth. The paper does not give a uniform scrap percentage for comparison, and the physical evidence is mainly profile, surface, and lot conformance.

This example illustrates that hot spot feeding and foam decomposition need to be controlled together under the same production conditions. The materials, density and temperature input to the model are consistent with those in the field, and the simulation can help locate the main problems; When new defects appear on site, check the input conditions again with physical objects and records. For other steel castings, the connectivity of ingate, final filling position and pattern density are still of reference significance, but the given temperature window and flow rate should be verified again according to the new 0 pieces and alloys.

The final process also lists foam bead preparation and patterning as operations that need careful control to stabilize density. Density variations in the same pattern change the quality of foam to be vaporized, so pattern inspection and casting records should correspond to the same batch. It is by reviewing this input that the reason for occasional defects after improving the runner is explained, and the subsequent field trial casting conditions are further determined.

P. Kaliuzhnyi、V. Doroshenko、I. Nebozhak,Archives of Foundry Engineering,26(1),45–51,DOI 10.24425/afe.2026.157968。 According to the original paper arrangement, with pictures quoted from the original paper.Original Paper · CC BY 4.0 · PDF