How Investment-Casting Shells Affect Alloy Nucleation: Oxygen Partial Pressure, Contact Time and Interfacial Reactions
Published:
2026-01-12
Differential scanning calorimetry, interface microanalysis and thermodynamic calculations were used to compare the nucleation behavior of yttria and zircon coatings on CMSX-4 nickel-base superalloy. The results show that the stability of ceramics depends on the actual atmosphere and reaction process, and the influence of raw material name on solidification structure is not enough to judge.
Figure 5: Surface and interface reactions of alloys on standard zircon/silica coatings, comparing with and without oxygen absorbers.
How Facecoat, Atmosphere and Thermal Cycle Affect Nucleation
Ceramic coating in investment casting is not only the contact boundary of molten metal, but also may change the initial nucleation conditions. For equiaxed castings with grain refinement, promoting nucleation may be beneficial. For single-crystal superalloys, nucleation after directional growth has been established will produce impurities and grain boundaries, which will impair creep or fatigue properties. The original paper revolved around the latter question: under what conditions does the shell surface become an effective heterogeneous nucleation site, and why ceramics, which were originally considered stable, still react with alloys.
The shape core is very sensitive to the interface structure and chemical composition. Local undercooling areas where the solidification front has not yet reached, or ceramic particles that fall off the shell during filling, may provide new nucleation sites. Settle drop test is commonly used to study wetting and metal-ceramic reaction in the past, and full size directional solidification is also studied directly. However, these methods are time-consuming, costly, and difficult to accurately compare nucleation temperatures under the same thermal history. The team therefore used differential scanning calorimetry to correlate controlled heating and cooling signals with microscopic evidence of the reaction interface.
The test alloy was as-cast CMSX-4. The control coat consists of standard zircon powder/colloidal silica system ZrSiO4/SiO2, pure yttrium oxide Y2O3, and mixed system of adding 4.5% yttrium oxide to standard coat slurry. The standard slurry also contains a defoamer and a wetting agent added in process proportions. The median particle diameter Dv(50) of the yttria-added particles was about 26.2. m These compositional and particle size conditions limit the material systems compared in this paper and are not a general evaluation of all yttrium-containing shells.
The researchers carried the sample in a high-purity alumina crucible with a volume of 85 μL and prepared a coating of approximately 20 - 40 μm thick on the inner surface. standard slurry is adde through a pipette and redundant slurry is discharged; pure yttria is apply in that form of an aerosol sol; The mixing group first added yttrium oxide particles to the standard slurry and then coated in the same way. The coating was dried at room temperature for 24 hours and subsequently calcined in air at 873 K for 1 hour. In this way, the preparation process can be fixed first, and then the difference between atmosphere and ceramic chemical composition can be investigated.
The CMSX-4 was machined into cylindrical specimens of 4 mm diameter, 1 mm thickness, and 70 - 90 mg mass, polished and cleaned with isopropyl alcohol prior to testing. The calorimetric equipment is Netzsch STA 449 F3 Jupiter with automatic sample changer and high temperature furnace up to 1923 K. After temperature equilibration, the standard thermal cycle heats from 1173 K to 1763 K at 10 K/min, then cools to 1173 K at 10 K/min. The first round of heating is used to promote contact between the alloy and the coating and eliminate the influence of the original as-cast structure.
The cumulative time period during which the sample temperature is above the solidus is defined as the liquid contact time, and the standard condition is 4980 s. To track how the reaction evolves over time, the pure yttria group is subjected to two shorter thermal cycles. one with a two-stage cycle at 1763 K for 10 min and a cooling rate of 25 K/min with a cumulative liquid contact time of 2280 s; The other method uses a single heating and cooling, holding for 5 minutes and the same cooling rate, with a cumulative contact time of 1140 s. Contact time is not equal to high temperature holding time alone.
Two conditions were adopted for atmosphere comparison: flowing 6-grade high purity argon and adding zirconium oxygen absorber OTS to further reduce oxygen level in furnace. The nominal purity of the gas was not directly taken as the actual oxygen partial pressure at the interface, but the calorimetric response and oxidation products were examined by comparing whether or not an oxygen absorbing device was installed. Oxygen can enter the interface from the furnace environment, and may also participate in the reaction between the original oxide and the melt, so the use of high purity argon alone is still not enough to ensure that the surface layer is completely inert.
The nucleation supercooling was calculated as ΔTn=Tm-Ts. Tm is the temperature corresponding to the melting endothermic peak in the heating process, Ts is the temperature at which solidification begins in the cooling process, and the latter is judged by means of the first derivative DDSC of the cooling curve. Figure 1 shows how these temperatures are determined. A minimum of five tests were performed for each material combination, some more often, to check for repeatability and dispersion. What is compared here is nucleation undercooling defined in this paper, which cannot be confused with temperature difference of all parts of casting, nor can it directly replace actual impurity defect rate.

To determine the cause behind the temperature change, the researchers mounted the solidified samples perpendicular to the metal-coating interface, polished them, and finally polished them with 0.25 μm colloidal silica. The interface was observed under Jeol 7000F field emission scanning electron microscope with backscattering imaging voltage of 20kV. Different reaction regions were identified by combining the elemental distribution of energy spectrum. Calorimetry gives when nucleation occurs, and cross-sectional morphology and elemental distribution are used to explain which reaction products may be involved in the process.
In addition, the coated crucibles containing the same alloy were placed into a Bridgman single crystal casting furnace for comparison. The furnace hot-zone temperature was 1793±15 K, with a holding time of 4500 s and a vacuum pressure of 10⁻⁴ mbar, followed by rapid transfer to room temperature. The crucible is placed on a ceramic plate 200 mm from the copper cooling plate, which therefore does not directly control the sample temperature. This test is used to compare the interfacial reaction layer formed by industrial furnace and calorimetric test, and statistical verification of the yield of complete single crystal castings is not performed.
Facecoat Stability Revealed by Undercooling and Reaction Products
Under the two atmospheres, the melting peak temperature Tm changes little, but the solidification onset temperature Ts changes significantly. For the standard ZrSiO4/SiO2 facecoat without the oxygen getter, the 5 measured nucleation undercoolings were 7, 20, 15, 32 and 39 K; After retrofitting, it is 109, 86, 97, 67 and 84 K. For the pure-yttria facecoat, values without the device were 13, 8, 9, 9 and 12 K, and those with the device were 26, 45, 67, 63 and 61 K. See Table I for complete temperature correspondence, and Figure 3 and Figure 4 for calorimetric curve and supercooling distribution.


| Surface and conditions | testing order | Tm / K | Ts / K | ΔTn / K |
|---|---|---|---|---|
| ZrSiO4/SiO2 with OTS | 1 | 1654 | 1545 | 109 |
| ZrSiO4/SiO2 with OTS | 2 | 1653 | 1567 | 86 |
| ZrSiO4/SiO2 with OTS | 3 | 1656 | 1559 | 97 |
| ZrSiO4/SiO2 with OTS | 4 | 1656 | 1589 | 67 |
| ZrSiO4/SiO2 with OTS | 5 | 1655 | 1571 | 84 |
| ZrSiO4/SiO2, no OTS | 1 | 1653 | 1646 | 7 |
| ZrSiO4/SiO2, no OTS | 2 | 1656 | 1636 | 20 |
| ZrSiO4/SiO2, no OTS | 3 | 1655 | 1640 | 15 |
| ZrSiO4/SiO2, no OTS | 4 | 1655 | 1623 | 32 |
| ZrSiO4/SiO2, no OTS | 5 | 1654 | 1615 | 39 |
| Pure Y2O3 with OTS | 1 | 1655 | 1629 | 26 |
| Pure Y2O3 with OTS | 2 | 1655 | 1610 | 45 |
| Pure Y2O3 with OTS | 3 | 1656 | 1589 | 67 |
| Pure Y2O3 with OTS | 4 | 1656 | 1593 | 63 |
| Pure Y2O3 with OTS | 5 | 1656 | 1595 | 61 |
| Pure Y2O3, no OTS | 1 | 1657 | 1644 | 13 |
| Pure Y2O3, no OTS | 2 | 1656 | 1648 | 8 |
| Pure Y2O3, no OTS | 3 | 1657 | 1648 | 9 |
| Pure Y2O3, no OTS | 4 | 1656 | 1647 | 9 |
| Pure Y2O3, no OTS | 5 | 1657 | 1645 | 12 |
This means that after decreasing oxygen level, the alloy must reach a greater undercooling before nucleation begins, and heterogeneous nucleation is more difficult to occur. The range for standard finishes was increased from 7 ° 39 K to 67 ° 109 K, and for pure yttria finishes from 8 ° 13 K to 26 ° 67 K. The change direction of the two materials is the same, but the numerical value and dispersion degree are different. Pure yttria does not exhibit the high nucleation threshold expected for low reactivity under normal argon; Its behavior needs to be understood in conjunction with the interface products actually formed.
A continuous alumina layer surrounding the alloy surface and whiskers in some areas were observed in the standard coating samples. The aluminum oxide layer at the contact between metal and surface layer is about 2.2 μm thick without oxygen absorption device and about 1.5 μm thick with oxygen absorption device. Whisker-like structure can be observed on the free surface at higher oxygen level. Hafnia oxide HfO2 was detected at the interface with or without oxygen absorbing device. Figure 5 in the original text compares the surface state, cross-section backscatter image and energy spectrum distribution, indicating that reducing ambient oxygen does not cause all reaction products to disappear at the same time.
The difference was more pronounced in the pure yttria group. Without oxygen absorber, alumina can be seen on the upper surface and at the edge of the bottom contact zone. Al2O3, YAG (Y3Al5O12) and YAP (YAlO3) co-exist in the edge reaction zone. in that cent of the bottom contact region, a reaction layer with a thickness of about 15 μm is for, which contains YAP, YAM (Y4Al2O9) and unreacted Y2O3, and HfO2 is detected. The products at the center and edge are different, indicating that the spatial conditions under which oxygen enters the interface can change the reaction path.

After adding oxygen absorption device, the upper surface of pure yttrium oxide alloy is relatively clean, aluminum oxide is no longer detected at the contact interface, only a small amount of reaction traces are left near the center, and discrete YAG particles with size less than 1 μm are observed. Figure 6 juxtaposes these results with those of the non-oxygen group. The inhibition of reaction layer and the increase of nucleation undercooling constitute two kinds of mutually supporting evidences: lower oxygen level improves the stability of yttrium oxide layer under this condition, and also weakens the promotion effect of interface on nucleation.
Both aluminum and hafnium in CMSX-4 have a strong oxidation tendency. Stable hafnium oxide can be detected in the reaction layer even if the hafnium content is only about 0.1%. For aluminum, the authors consider that the formation of alumina is firstly related to oxygen entering from the periphery of the furnace according to the fact that alumina is mainly located at the edge of the contact zone rather than in the center. The edge-generated alumina then reacts with yttrium oxide to form YAP, which in turn reacts with alumina to form YAG, so that multiple oxides can coexist in the edge region rather than a single, uniform layer of product.
In the central region, there is less oxygen in the environment, so another reaction path is proposed: aluminum in the melt interacts with yttrium oxide to form YAM and YAP successively, and yttrium enters the melt; YAM can continue to transform to YAP, and YAP can evolve to YAG in the following stages. Equations [2]-[7] describe these possible chemical pathways. YAM distributed around YAP and adjacent metals of YAP in microstructure, which supported this order judgment. They are explanations of the interface reaction process and cannot be assumed to follow exactly the same path at each location by the final cross section alone.
The results of the reduced contact time further tested this interpretation. when that cumulative liquid contact time is 2280 s, the co-existence of YAG and YAP can be seen in the cent interface, YAG is close to the metal, YAP is closer to the coat, and YAP, YAM and Y2O3 still exist locally, which indicates that the transformation is not complete. When the contact time was shortened to 1140 s, YAP particles separated from each other mainly existed in the center, multiphase mixed zone still existed in the edge, YAG was almost absent. FIGS. 7 and 8 thus relate the successive appearance of the reaction products to the change in the degree of supercooling.


Correspondingly, the nucleation supercooling of 2280s group is 16, 25, 33, 19, 50 K, and that of 1140s group is 28, 31, 31, 46, 80 K. The Tm and Ts of each time are listed in Table II. With a shorter contact time, the subcooling interval changes from 16 ° 50 K to 28 ° 80 K. The authors associate this with limited reaction time, reduced reaction products and reduced chances of formation of effective nucleation sites. Since the short-time scheme uses different thermal cycles and cooling rates simultaneously, the corresponding test conditions need to be preserved when applying these results, and only the number of seconds cannot be extracted as a general process value.
| duration of exposure | testing order | Tm / K | Ts / K | ΔTn / K |
|---|---|---|---|---|
| 2280 s | 1 | 1660 | 1644 | 16 |
| 2280 s | 2 | 1659 | 1634 | 25 |
| 2280 s | 3 | 1659 | 1626 | 33 |
| 2280 s | 4 | 1658 | 1639 | 19 |
| 2280 s | 5 | 1660 | 1610 | 50 |
| 1140 s | 1 | 1657 | 1629 | 28 |
| 1140 s | 2 | 1659 | 1628 | 31 |
| 1140 s | 3 | 1658 | 1627 | 31 |
| 1140 s | 4 | 1659 | 1613 | 46 |
| 1140 s | 5 | 1658 | 1578 | 80 |
When 4.5% yttrium oxide is added to the standard zircon/silica coating, the nucleation undercooling reaches 22.6 - 86 K, which is higher than 8 - 13 K of pure yttrium oxide and 7 - 39 K of undoped standard coating under ordinary argon condition. This result indicates that the interface behavior of the two materials after mixing is not a simple superposition of their individual performances. Under this experimental condition, the effect of mixed coating on the nucleation of Ni-based γ grains is weakened, but it cannot be inferred that the same result will be obtained with any amount of mixed coating.
A continuous alumina layer with a thickness of about 10 μm was formed on the surface of the mixed coating sample. At the edge of the contact region, a YAG network embedded in the alumina layer and dispersed ZrO2 particles were observed; the same reaction products were not found at the center. The comparison of locations in Figure 9 illustrates once again that the local chemical environment affects material stability. Therefore, it is emphasized that the interfacial reaction of alumina should be considered when analyzing the effect of yttrium oxide addition, and yttrium oxide should not be regarded as a constant protective layer.

A 20 μm thick reaction layer containing YAP, YAM and residual Y2O3 was formed at the center of pure Y2O3 contact interface of commercial Bridgman furnace sample, and Al2O3 and YAG existed at the periphery. Its thickness, composition and morphology are close to those of calorimetric samples without oxygen absorption device. The comparison of FIG. 10 supports the calorimetric method as a tool for screening the reactivity of the topcoat. CMSX-4 master alloy of the same origin was also used in type 2 test, and the oxygen concentration of the raw material was less than 1 ppm; This indicates that low oxygen content in raw materials and low oxygen content in furnace interface belong to different links.

To determine whether these reaction products are stable phases or intermediate stages, the authors modified a Kampmann–Wagner model, placing one or more spherical oxide particles in a spherical region representing the CMSX-4 melt. The change of particle radius with time is controlled jointly by liquid solute diffusion, particle radius and normalized reaction free energy. The original model formula [1] is written as dr/dt=(D/r)·(ΔGr/RT). According to the sign convention in this paper, negative driving force corresponds to particle shrinking, positive value corresponds to growth, and zero value corresponds to balance.
The model uses the activity of oxygen and metal elements in liquid phase to calculate the driving force of reaction. The activity information is provided by TCNI8 database. At each step, the element conservation calculation is performed again according to the generation or dissolution of solid particles, the liquid phase composition is updated, and the oxide which may be stable is judged through the TCOX11 database. It is assumed that there is no nucleation kinetic barrier when new phases are introduced. This results in a solution-reprecipitation process that varies with local composition, rather than a fixed reaction layer model in which one product is specified in advance and allowed to grow continuously.
In the pure-yttria/CMSX-4 calculation at 1763 K, yttria remains stable at a liquid-phase oxygen mole fraction of 10⁻⁴; At 10⁻³, yttria begins to destabilize; yttrium and oxygen dissolved in the melt promote the formation of YAG, YAM and YAP, with YAG becoming the main product in the model. Figure 11 corresponds to a trend consistent with the oxygen uptake test. The two values here are the oxygen mole fraction of the melt used in the calculation, not the oxygen partial pressure of the gas in the furnace, nor should they be directly used as the set value of the atmosphere of the production furnace.

Calculation of mixed coating containing 4.5% yttrium oxide shows that ZrSiO4, SiO2 and Y2O3 are dissolved gradually, making Zr, Si, O and Y enter liquid phase. YAG is for in that early stage, and then dissolves with the change of chemical environment; Alumina continues to grow and become the main phase, while zirconia appears tetragonal phase first, and then grows with fluorite structure. The process of FIG. 12 explains why alumina, YAG, and zirconia were eventually observed in the experiment, and also shows that the combination of phases in the final cross-section is not a complete representation of the earlier reaction history.

This study puts nucleation temperature, interfacial reaction layer and dynamic phase evolution in the same chain of evidence. The core conclusion is that the stability of the coating is closely related to the availability of oxygen, active elements in the alloy, contact time and mixed oxide reaction. Decreasing oxygen level or limiting reaction development can increase the undercooling required for nucleation in the studied systems. However, some controlled reaction products may be used as nucleation promoters when it is desired to promote equiaxed grain refinement, and the evaluation direction depends on the desired microstructure of the casting.
Calorimetric method is easy to compare thermal response of small sample repeatedly, but it can not provide contact angle information in sessile drop test at the same time. The kinetic obstacle of nucleation is omitted when new phases are introduced into the model. CMSX-4 and specified ceramic systems are the material objects of the original thesis, which are suitable to provide basis for the screening of single crystal superalloy coating, the evaluation of impurity effect and the study of nucleation mechanism. When it is used in other alloys or shell formulations, it still needs to be verified by corresponding materials, atmospheres and thermal history, so that the interface screening results can be converted into actual casting technology.
Richa Gupta、Ben Goodyer、Dmytro Shevchenko、Roger Reed、Joseph Moses、Nils Warnken、Owen Draper、Nick Green; Metallurgical and Materials Transactions A,57,1723–1735; DOI:10.1007/s11661-025-08057-z。 This paper compiled according to the original paper, maps and data using CC BY 4.0 authorization.Original Paper · PDF · CC BY 4.0 ·
Related News