Activated-Carbon-Assisted Microwave Dewaxing of Ceramic Shells: Heating Uniformity, Wax Removal and Cracking
Published:
2025-12-12
The microwave dewaxing of 30 samples with the same geometry was studied by adding activated carbon absorbing coating between wax pattern and ceramic shell. Results Surface temperature, wax recovery, and shell cracking were recorded simultaneously, showing an average dewaxing rate of 93.76%, while integrity was still evaluated in conjunction with residual moisture and localized heat buildup.
Figure 4: Ceramic shell on tripod and wax tray below.
Susceptor Coating, Three-Layer Shells and a Common Dewaxing Test
The dewaxing stage of investment casting requires rapid melting and drainage of wax while avoiding wax expansion and local temperature differences that can crack the shell. Conventional steam dewaxing and combustion fast dewaxing each have equipment, energy, and wax recovery requirements. Microwave dewaxing attempts to change the location of heat entering the shell system. Cavero Luján et al. set a wave-absorbing layer on the surface of the wax pattern with small sculpture geometry as the object, so that after the microwave passes through the ceramic shell with low loss, the electromagnetic energy is converted into heat close to the wax surface by the wave-absorbing material.
The key to this method is not just raising the temperature. If the absorbing layer is unevenly distributed and the local temperature rises too fast, hot spots, cracks and even spontaneous combustion may occur in sharp corners, concave cavities and weak areas. The research team has previously examined graphite and titanium oxide combinations, and this time activated carbon was selected to examine whether it could produce more gradual and stable heating and expel wax from complex geometries. In order to distinguish the thermal response of the coating itself from the dewaxing behavior of the wax-shell system, the characterization of the absorbing material was separated from the actual shell test.
the microwave absorb coating is prepare from 15% by mass of active carbon powder and 85% by mass of colloidal silica into a suspension, and a continuous lay is obtained by brush coating. the colloidal silica both aid in that distribution and adhesion of the powder and constitute the binder phase in the coating. The raw materials are analytically pure activated carbon and Hispasil 1731 silica sol listed in the paper. This ratio refers to the composition of coating suspension, the study did not use "all shell containing 15% activated carbon" as the shell preparation scheme, the ceramic body is still prepared according to the subsequent refractory slurry and sand scattering process.
characterization of that material: first, the carbon, hydrogen and other elements of the original activate carbon were determined by the modified Dumas combustion method use a Thermo flash EA 1112 elemental analyzer. Then the same coating was brushed on ceramic support with an area of about 1 cm², and BMW samples without microwave treatment and AMW samples after 70 s microwave treatment were kept respectively for scanning electron microscopy and energy spectrum comparison. This phase, in which the coating is exposed to air and not to wax, is used to analyze changes in structure and composition of the coating before and after treatment.
The scanning electron microscope was JEOL JSM 6300 with Oxford 6699 ATW energy dispersive spectrometer. Table 2 gives an accelerating voltage of 20 kV, an EDS live acquisition time of approximately 50.01 s and a real time of approximately 64.45 s. The response of the independent coating was recorded by thermography at the same time as the study, but the surface temperature of the intact shell specimen was used as the basis for discussion of actual dewaxing. Heat absorption, contact state of wax and heat transfer of shell will change the temperature rise process under independent coating conditions.
The actual dewaxing uses 30 wax molds, each weighing 43 g, cast from the same silicone rubber mold. The wax composition is 70% yellow beeswax, 20% paraffin wax and 10% rosin. The melting temperature range of these components is given in Table 3. The model has geometric features such as sharp corners, concave cavities and hollows, and can observe thermal response at different positions. The sprue and sprue cup are manufactured using another silicone rubber mold and manually assembled with the main body, keeping the size and wall thickness consistent as much as possible.

Before the wave absorbing layer is coated, the wax pattern is cleaned first, and the shellac isolation layer is brushed on the surface. Insect film was prepared with 95% ethanol at the given 3:1 volume ratio and dried at room temperature for about 10 min after coating to allow solvent evaporation and improve adhesion of subsequent layers. Then brush activated carbon-silica sol suspension evenly, keep the concave surface of the pouring cup as the wax outlet, dry the absorbing layer for about 15 minutes, and then start conventional ceramic shell making. FIG. 2 shows the sequential composition of the wax pattern, the wave-absorbing layer and the refractory layer.

The ceramic shell was prepared in three layers. The first layer slurry adopts 70% Molochite refractory powder and 30% silica sol, and fine Molochite (50/80 DD) is scattered; The second layer is adjusted to 60% refractory powder and 40% silica sol, and the same fine sand is still used; The third layer consists of 50% refractory powder and 50% silica sol, and coarse 16/30 DD sand is used instead. the specification of that refractory pow is less than 200 mu m, and the concave surface of the pouring cup which need to be reserved is also not coated.
| shell | mas ratio of refractory powder | Silica sol mass ratio | sand specification |
|---|---|---|---|
| Tier 1 | 70% | 30% | Molochite 50/80 DD |
| Layer 2 | 60% | 40% | Molochite 50/80 DD |
| Layer 3 | 50% | 50% | Molochite 16/30 DD |
The shell-building environment was maintained at 22–25 ℃ and 50%–60% relative humidity. The drying time for the first layer is 12 - 24 h, and each subsequent layer is dried for about 2 h, and forced ventilation is used. The author keeps the composition and fabrication method of the conventional ceramic shell, and mainly changes the absorbing interface near the wax pattern, so that the experiment revolves around the effect of activated carbon coating. Residual moisture, another influencing factor, was compared at two levels in the final shell.
The microwave equipment is Panasonic NN-GT 45KW multimode cavity, operating frequency is 2.45GHz, maximum power is 1100W, cavity size is about 247×359× 362mm, with 7 power adjustment. 30 samples are processed one by one, each sample is placed in the center of the turntable according to the uniform procedure of 1100 W and 70 s, and the position is kept consistent. The mold shell is suspended by a tripod support, and a wax collecting tray is arranged below, so that the molten wax can flow out from the reserved outlet instead of staying in the heating area.
Temperature is measured by PCE-TC33N thermal imager with image resolution of 220×160, spectral range of 8 - 14 μm, thermal sensitivity of no more than 70 mK, nominal accuracy of ±2 ° C or ±2% of reading. Open the door immediately after each irradiation to obtain the thermal image. Figure 3 shows the measurement process. In this paper, the maximum surface temperature of the thermograph is used as the main analysis variable, because it reflects the position where the heat accumulation is most likely to occur. The surface response near the end of treatment is measured rather than a continuous temperature record at all locations inside the mold.

The dewaxing effect is checked by weighing and visual inspection simultaneously. Each sample was weighed separately before and after microwave treatment, and the recovered wax in the wax collection tray was also weighed separately to calculate the wax discharge and recovery; Structural inspection records of cracks, local collapse, hot spots and spontaneous combustion. Figure 5 connects sample preparation, processing, thermography, and weighing in series. When evaluating the same sample in this way, it can not only see how much wax is discharged, but also whether the shell is still suitable for undertaking subsequent processes, avoiding evaluating all process performances only with high dewaxing rate.

Wax Removal, Shell Integrity and Residual Moisture
Elemental analysis of the original activated carbon powder showed that carbon 85.37% and hydrogen 1.41%. The energy spectrum of microwave absorbing coating was measured by another method, and the influence of binder and ceramic support was included: the carbon content of untreated BMW sample was 75.68%, oxygen content was 17.45%. After treatment, carbon content in AMW is 68.54%, oxygen content is 19.05%, silicon content is 10.18%, aluminum content is 1.66%. Micrographs and corresponding spectra are given in Fig. 6 and Fig. 7.


The authors suggest that the decrease of carbon content and increase of oxygen content after treatment are related to surface oxidation to a certain extent, and the increase of substrate related elements may be due to thinning or microcracking of the coating. The material undergoes a detectable surface change, but retains its absorbing heating function. The elemental analysis of powder combustion and local energy spectrum of coating answer the questions of raw material composition and surface state respectively, so the three groups of carbon content belong to the data under different samples and test conditions, and this measurement background is retained when comparing.
| coating sample | Carbon/ wt.% | Oxygen/ wt.% |
|---|---|---|
| BMW, pre-treatment | 75.68 | 17.45 |
| AMW, Post-Process | 68.54 | 19.05 |
For 30 ceramic shells treated with the same 70 s, 1100 W program, the maximum surface temperatures recorded by thermal imaging ranged from 87.9 to 126.1 ℃. The temperature of the whole sample increases gradually, and most of the samples are heated evenly. Figure 8 summarizes the individual tests and Figure 10 maps the maximum temperature of each sample to the percentage dewaxing. Temperature differences still occur under the same equipment settings, reflecting geometric details, coating uniformity and residual moisture factors acting together on the actual thermal response.


The average wax excretion rate was 93.76% and the standard deviation was 5.53%. Of the 30 samples, 19 achieved at least 95% wax rejection, 17 of which met both the high dewaxing rate and the absence of structural defects. The higher average value indicates that this set of absorbing layers can support fast wax melting and expulsion, but the differences between samples still exist; The double condition passing number further distinguishes the requirements of the two stages of "wax discharge" and "shell intact after discharge".
Hot spots and spontaneous combustion were also recorded separately, with 1 in 30 cases each, corresponding to 3.3% each. In contrast, the cumulative number of cracks in the shell is higher. 17/30, i.e. 56.7%, is used to summarize the successful results of complete shell or double conditions, indicating that the microwave absorbing ability of the material has been supported, and the reliability of the whole shell-dewaxing combination still has room for improvement. These itemized data reflect the experimental effect more completely than the summary of "efficient and stable" in the abstract.
| index | result |
|---|---|
| average wax removal rate | 93.76% |
| wax discharge rate standard deviation | 5.53% |
| Wax removal rate at least 95% | 19/30 |
| High dewaxing rate and no structural defects | 17/30(56.7%) |
| hot spot record | 1/30(3.3%) |
| autoignition record | 1/30(3.3%) |
| Maximum surface temperature range | 87.9–126.1 ℃ |
There is a clear trend observed between temperature and shell condition. Microcracks are more likely to appear at sharp edges and deep concave cavities when the temperature exceeds 115 ℃. At temperatures around 95 - 105 ° C, a good balance is achieved between wax removal and shell integrity. Increasing the maximum temperature did not consistently bring better dewaxing effect, but increased damage in some geometrically concentrated areas. Therefore, the author regards the uniformity of temperature field and the gradual degree of temperature rise process as important technical indexes as temperature peak value.
Figure 9 shows physical and thermal images of two specific specimens: No. 13 was able to complete dewaxing and remain crack-free, and No. 15 showed visible cracks at the shell edge. Corresponding the damage position to the thermal image, we can observe whether there is heat concentration at the same time in the sharp corner area. The evidence here comes from the designated specimen and post-treatment surface examination, indicating that the same irradiation program does not have uniform effects on different local locations, and also provides specific clues for subsequent adjustment of coating thickness and shell strength.

The residual moisture was divided into 2 groups: 0.6% group (10 pieces), 6 pieces cracked (60%); 0.8% group 20 pieces, 7 pieces cracked, the proportion is 35%. Since the outcome variable is crack presence or absence, Fisher's exact test was used and p = 0.26 was obtained. Figure 11 retains the proportions of the two groups. The observation direction of samples supported that the higher moisture group had fewer cracks, but the statistical test did not reach significance, and the sample sizes of the two groups were also different.

| residual moisture | number of samples | Number of cracked units | cracking ratio |
|---|---|---|---|
| 0.6% | 10 | 6 | 60% |
| 0.8% | 20 | 7 | 35% |
The authors suggest that proper residual moisture may buffer the local temperature rise through its dielectric absorption and heat exchange, so that the heat can be dispersed more smoothly. Localized heating may be faster at lower moisture levels, and stronger thermal gradients increase cracking tendencies. This interpretation is consistent with this group of observations, but needs to be tested with larger samples and finer moisture control. 0.8% is a comparative level in this test and is not a uniform optimal value that has been verified for all shells, equipment, and 0 pieces.
The mechanism of activated carbon is explained by means of existing dielectric studies. The complex dielectric constant quoted in the original paper is about εr=14.69-j6.06 at 30 ℃ and 14.47-j5.37 at 70 ℃, where the imaginary part represents the loss component. The corresponding loss factor decreases slightly with temperature, with a reported slope of approximately −0.017 ℃⁻¹. According to this, the author explains that activated carbon has a certain self-limiting temperature rise trend: when the temperature rises, the absorption loss does not continue to strengthen to the same extent, which is beneficial to reduce thermal runaway.
These dielectric values are derived from material studies cited by the author. The 30-piece shell test mainly provides verification of temperature, dewaxing and integrity. The mechanism comparison between graphite and activated carbon is also based on previous experiments and literature. It is considered that the loss of graphite increases with the temperature, and the local heat accumulation is more likely to occur. titanium oxide play a more dielectric regulating role. The current test uses a uniform activated carbon formulation and does not have the same number of graphite and titanium oxide replicates in the same batch of 30 units.
From the heat transfer process, the wax needs to melt from the position of contact with the absorbing layer and form a discharge channel, and the shell bears the load caused by temperature difference and residual wax expansion. If the absorbing layer is locally too thick, the powder distribution is uneven, or the structure near the exit is unfavorable, the temperature rise in one place can be faster than that in other areas, resulting in additional thermal stress. Based on this, the author considers coating thickness, sand uniformity and internal geometry as the key points of subsequent optimization, especially the coupling effect between electromagnetic field distribution and shape details.
The 3-layer shell was the fixed preparation condition for this experiment. It is suggested that the layers can be increased, the strength and pore structure of refractory layer can be improved, or the shell can be strengthened by referring to plant fiber. Microwave power and time also need to be adjusted with model complexity. These belong to the follow-up improvement direction, the unified procedure of 30 pieces in this paper is still 1100W, 70s. Separating the recommendations from the test conditions that have already been completed allows you to see the range supported by the current data and the process space that remains to be validated.
Geometric scale also affects promotion. The wax pattern is 43 g, using the same shape and basically the same clamping position; Larger shells have more complex field distributions, temperature differences and wax removal paths, and the same effect cannot be inferred only by extending the irradiation time in proportion to mass. It is suggested that the different size and morphology should be further examined, and the effect of microwave absorbing treatment on the thermodynamic properties of subsequent metal casting and shell and solidification stage should be studied. This paper mainly verifies the dewaxing stage, and does not provide a complete set of control data on the quality of the final metal castings.
This study shows that placing an activated carbon absorbing layer between wax and ceramics can achieve higher wax removal rates in short-term microwave processing, and most samples do not have hot spots or spontaneous combustion. At the same time, the lack of statistically significant differences in shell integrity, moisture content, and the range of tests for a single small geometry indicate that the method still needs to be refined around stability. The technical inspiration is to evaluate the absorbing material, shell structure, geometry and moisture state as a combination process, rather than pursuing higher power or higher temperature alone.
For shell dewaxing research, the combined indexes adopted in this paper can be used for reference: uniform program to ensure comparison within the group, thermal image to locate local heat accumulation, weighing before and after and wax collection to evaluate discharge, and crack inspection to evaluate structure retention. This not only retained the average dewaxing performance of 93.76%, but also clearly presented the actual results of 17 successful double conditions, which provided a verifiable starting point for improving shell quality and heat distribution in the next round.
Rut Cavero Luján、Itahisa Pérez Conesa、Jose Antonio Aguilar Galea; International Journal of Metalcasting,20,3542–3555; DOI:10.1007/s40962-025-01830-1。 This paper compiled according to the original paper, maps and data using CC BY 4.0 authorization.Original Paper · PDF · CC BY 4.0 ·
Related News