Reducing Flash and Gas Porosity in Die Castings: Simulation and Production Validation of Local Runner Modifications


Published: 

2025-11-18

In view of the flash, aluminum adhesion and local wear of aluminum alloy window frame bracket in the early stage of use of the mold, the flow-heat transfer simulation was used to reproduce the field working conditions, and two schemes of closing branch and increasing runner necking were compared. The modification effect was verified by infrared temperature measurement, casting appearance and internal pore inspection.

Figure 1: Case study: Two kinds of aluminum alloy window frames assembled with bolts.

Figure 1: Case study: Two kinds of aluminum alloy window frames assembled with bolts.

Modeling Flow and Cyclic Heat Transfer from Production Defects

The filling, solidification, opening and spray cooling of high-pressure die casting occur repeatedly in a short period of time, and the metal flow and mold temperature field are therefore closely linked. Local overheating not only affects solidification, but also changes mold expansion, adhesion between molten aluminum and mold surface and fit state near parting surface. Campanella et al. study of aluminum alloy window frame bracket, at the beginning of the production will appear at the same time flash, adhesive aluminum and local collapse. Based on these practical problems, it is analyzed whether mold filling stability and mold thermal balance can be considered through limited runner modification.

The object of study consists of two support geometries, which are finally assembled by bolts. The assembly relationship is shown in Figure 1. Production uses OMS 550 die-casting machine, clamping force is 5600 kN, maximum injection force is 520 kN, annual production target is 500,000 pieces. The casting material is EN46100 (AlSi11Cu2Fe), and the mold adopts the corresponding H13 material configuration in the database. This case is of high pressure die casting of aluminum alloy, and the flow rate, cycle time and die boundary conditions in the study are determined around this production line.

The total length of a single on-site cycle is 34.2 s. Filling and solidification are completed in about 10 s, followed by mold opening, picking up parts by robot arm, spraying mold release agent and blowing, and then entering the next cycle. Table 2 further lists the stages as solidification 9.3 s, mold opening 12.8 s, spray interval 6.0 s, mold closing 3.9 s, casting delay 1.0 s and metal pouring 1.2 s. The simulation followed this schedule to keep the heat input and heat loss at each stage consistent with the field beat.

Table 2: Stages and duration of a single die casting cycle
stageTime/s
solidification9.3
die sinking12.8
Spray Interval6.0
die assembly3.9
casting delay1.0
metal pouring1.2

After approximately 2000 cycles of mold operation, visual inspection has revealed significant defects. The flash in Figure 3 is mainly characterized by the escape of molten aluminum along the parting gap of the die, forming a thin sharp edge that exceeds the product profile and requires additional deburring. The light areas of FIG. 4 are aluminum adhering to the die surface, which changes the surface heat transfer and contact conditions as cycles accumulate. The casting defect and mold damage should be recorded together to avoid deducing one isolated process parameter from the flash of finished product.

Figure 3: flash on the casting of the reference scheme, red circles mark the defect location.
Figure 3. Flash on the casting of the baseline scheme, with red circles indicating the location of the defect.
Original Figure 4: Aluminum adhesion area of the die surface of the reference scheme. Red arrows indicate the metal adhesion position.
Figure 4. Aluminum sticking area of the die face of the benchmark scheme, with red arrows marking the metal attachment locations.

Small forming parts of the mold also appear local collapse. The author relates this phenomenon to fatigue and plastic deformation caused by repeated thermal expansion and contraction, and to the change of local contact pressure after bonding aluminum. Waterless mold release agents used in the field help mitigate cooling thermal shock, but their inhibition of aluminum residue accumulation is still limited. These observations suggest that it is necessary to consider die surface temperature difference, aluminum impact and cyclic loading simultaneously, rather than attributing all problems to insufficient spray or simple mold material strength problems.

Two modules of CASTLE software were used in numerical study. CASTLEBODY Computational Fluid Dynamics Analysis of Metal Flow and Air Distribution in Mold Filling CASTLETHERMO uses the finite element method to analyze the temperature, cooling rate and spatial temperature difference in the cycle. The former identifies stream-strand encounters, local high velocities and entrainment regions, while the latter tracks hot spots and thermal imbalances between stationary and moving modes. Type 2 results are combined to determine whether the runner modification improves both flow and heat load distribution.

The flow model consists of two phases, metal and air, with the continuity equation being Γ·u=0. The momentum equation retains the terms of inertia, pressure, viscosity, gravity, and surface tension, corresponding to equations (1) and (2), respectively. The liquid-gas interface is tracked by the transport equation for volume fraction α. Equation (3) contains an artificial compression velocity term to keep the interface clear. Mixture properties such as density are weighted by the volume fractions of metal and air, enabling the simulation to update the two-phase interface as the mold fills, rather than just mapping the region eventually occupied by metal.

The transient heat conduction equation is used for heat transfer of the mold. The original formula (4) is ρ s·cp·T/t =·(ks T)+ Q, where ρ s, cp and ks are the density, specific heat and thermal conductivity of the mold respectively, and Q is the internal heat source. The heat input from molten aluminum to the mold and the heat dissipation in cooling channel, mold opening and spraying are considered in the model. This allows you to track the temperature rise and fall at the same point in a continuous cycle, and you can also compare the temperature differences in different die surface areas at the same time.

The geometry is imported into STEP format and discretized using hybrid meshes. Hexahedral elements are used in the inner part of the mold, and thinner tetrahedral and prismatic elements are used in the thin wall, rounded corner, ingate and areas where large temperature gradient is easy to occur. The average unit size of the main body is about 4 mm, and the key area is refined to 0.5 mm; At least 2 layers of units shall be arranged in the thin section and overflow port thickness direction, and at least 3 layers of ingates shall be arranged. The final model had approximately 12 million units, and Figure 6 shows the spatial relationship of the mold, casting, and cooling circuit.

Figure 6: Overall structure of the model: fixed mold, moving mold, casting and cooling circuit.
Fig. 6 Overall structure of the mold: fixed mold, moving mold, casting and cooling circuit.

The model contains cooling channels with a diameter of 8 mm, and a grid of about 0.5 mm is also used near the channels to resolve local temperature gradients. The cooling-water temperature and flow rate were set to 35 ℃ and 3 L/min. From the flow rate and geometry, the software calculated a heat-transfer coefficient of approximately 21900 W·m⁻²·K⁻¹. The authors also checked the result using the Nusselt-number relation h=Nu·k/Dh and the Dittus–Boelter correlation Nu=0.023Re⁰·⁸Prⁿ, obtaining 21939 W·m⁻²·K⁻¹. The two values are close; these relations correspond to Eqs. (6) and (7) in the paper.

The injection motion is input according to the field punch travel-velocity curve. the speed is gradually increase in that slow injection stage, so that the aluminum liquid advances along the pressure cham; After the stroke reaches about 300 mm, it enters the rapid injection, and the maximum punch speed is about 1.5 m/s. The end of the stroke decelerates sharply and then enters the pressurization phase. Figure 7 retains this boundary condition. The punch velocity is a machine motion parameter, while the metal velocity in the gate and local runner is determined by the channel section, filling state and flow calculation, which are used to describe the response of different positions respectively.

Figure 7: Punch stroke-velocity curve used for simulation.
Figure 7 Punch stroke vs. velocity curve used for simulation.

In thermal control, mold target temperature is set to 105 ℃, and cooling channel automatically stops when it reaches this condition to reproduce field temperature control logic. Twelve die-casting cycles were calculated continuously, and two monitoring points were selected in fixed die and two monitoring points in moving die to check whether the peak temperature still increased with the cycle. By about the 10th cycle, the temperature peak has stabilized, so the subsequent comparison mainly focuses on the spatial distribution of the thermal stabilization phase to avoid mixing the cold mold start-up with the temperature state of stable production.

Comparing Runner Modifications through Temperature and Porosity Measurements

The baseline scheme still has significant spatial temperature differences after thermal stabilization. Two paths A and B were set up in the movable die, and two paths C and D were set up in the fixed die, covering the upper area far away from the runner and the lower area near the central runner respectively. The calculated temperature plot of Figure 10 shows that the imbalance exists both within the same mold half and between the stationary and moving molds. The comparison of path average temperatures shows that the difference between the upper and lower regions of the same mold half is about 50 ℃, which constitutes the basis for explaining the differential thermal expansion and local damage.

Figure 10: Pre-spray die surface temperature after thermal stabilization of baseline scheme, A-D is analysis path.
Fig. 10 Temperature of die surface before spraying after thermal stabilization of benchmark scheme, A-D are analysis paths.

To verify temperature predictions, FLIR T6xx infrared cameras were used in the field to collect mold surface temperatures during the thermal stabilization phase prior to mold release and blowing. The camera has a resolution of 640×480, a spectral range of 7.5 - 14 μm, and an accuracy of ±1 ° C or ±1% of the reading, calibrating the emissivity before measurement. The measured temperatures are also extracted along paths A ′, B ′, C ′, D ′. Figures 12 and 14 correspond the measured distributions to the simulated curves, maintaining consistency in comparison locations and sampling phases.

Figure 12: Measured infrared temperature plots of fixed and mobile models for the reference scheme.
Figure 12 Measured infrared temperature plots of the fixed and mobile stents of the baseline protocol.
Figure 14: Comparison of measured and simulated temperatures on the four paths of the baseline scenario.
Figure 14 Comparison of measured and simulated temperatures on four paths of the baseline scenario.

The average temperature difference between the measured temperature and the simulated temperature is about 6 ℃, and the corresponding average error is about 2%. Infrared measurements also showed a temperature difference of approximately 50 ℃ between upper and lower regions, and local hot spots reaching approximately 350 ℃ near the central runner and injection point. Both the magnitude of the model error and the spatial location of the defect correlation are preserved, allowing subsequent comparisons to be based on benchmarks that have been supported by field temperatures. The role of 12 simulation cycles is to determine the thermal stability state, and the observation of the mold after about 2000 production cycles reflects the occurrence of actual damage.

The flow calculations also show that the local metal velocity in the center runner is close to 80 m/s, corresponding to the area where the aluminium sticking is evident, see Figure 15. Although the baseline filling can be completed on the whole, there is air entrapment near the upper row of supports. The temperature field explains the mismatch between hot spots and thermal expansion, while the flow field supplements information about high-speed impacts, stream confluence, and entrainment. Therefore, the goal of modification is to improve the two kinds of conditions instead of reducing the average temperature of the mold to a certain value.

Figure 15: Distribution of filling velocity and Plane_A section of central runner.
Fig. 15 Distribution of filling velocity and Plane_A section in center runner.

The modification is constrained by site conditions, and the author hopes to retain most of the mold structure and existing production rhythm. The first CC (Closed Casting) closes the upper supply branch to redistribute the aluminum path and heat load and reduce the imbalance between the upper and lower mold halves. The second scheme, CCB (Closed Casting with Bottlenecks), builds on that design by adding local constrictions near the ingates and other runner positions to regulate the flow fronts and their merging sequence. Figure 16 shows two configurations, the necking local mark width is 3.7 mm, and the adjacent channel width is 9.5 mm; The original protocol served as a common control.

Original Figure 16:2 modifications: CC closed supply branch; CCB adds necking on this basis.
Fig. 16 Two modifications: CC closed supply branch; CCB adds necking on this basis.

Closing the slip roads alone does not solve all the problems. Fig. 17 compares the same filling time of 0.05 s: CC improves the flow supply of the upper left and right corner brackets, but makes the metal front meet locally too early, enclosing the internal space in advance, and causing a larger air stagnation area above the center runner. The degree of filling at this moment is even lower than that of the reference solution. This comparison shows that seemingly reasonable changes in the direction of heat load distribution may still introduce new flow problems that need to be further screened by liquid-gas two-phase calculations.

Original Figure 17: Filling state and air porosity prediction of original scheme, CC and CCB at 0.05 s, with display threshold of 5%.
Figure 17 The filling state and air porosity prediction of the original protocol, CC and CCB at 0.05 s, showing that the threshold value is 5%.

The flow front is more stable and premature collision and air accumulation are reduced after CCB increases the local constriction. When the results were displayed at the original 5% air porosity threshold, the predicted air porosity for almost the entire casting was below this threshold. This value is the display and comparison limit of simulation results, corresponding to spatial distribution, rather than the total porosity obtained by batch statistics of the whole product. The study then continued with an internal inspection of the actual casting to verify that this flow improvement corresponded to better solid quality.

Another comparison uses oxidation formation index, which ranges from 0 to 1, indicating no obvious oxidation defect tendency and severe state respectively. The local peak of the original scheme and CC in FIG. 18 is close to 1, while the index of CCB is about 0.5. The authors believe that more stable filling and less gas involvement reduce the precursor conditions for related defects. This index is a prediction index of software, which is different from the mass fraction of oxide film. It is used to compare the relative performance of three kinds of runners.

Figure 18: Prediction of oxidation formation index for 3 scenarios: Original, CC and CCB.
Fig. 18 Prediction of oxidation formation index for three schemes: original scheme, CC and CCB.

Thermal analysis continues to check whether CCB also improves the temperature profile. Figure 20 shows the pre-spray die surface temperature after stabilization, and Figure 21 extracts the results along the same four paths as the baseline. The temperature difference between the upper and lower regions of the movable mold is reduced to 12.6 ℃, and that of the fixed mold is about 22 ℃, which is lower than that of the reference scheme by about 50 ℃. Compared with only looking at the average temperature of the whole mold, this group of data directly indicates that the local heat load distribution has been improved, and also corresponds to the reduction of the inconsistency of the thermal expansion of the two halves.

Figure 20: Temperature distribution of pre-spray die surface after CCB thermal stabilization.
Fig. 20 Temperature distribution of the die face before spraying after CCB thermal stabilization.
Figure 21: Temperature curves and regional averages for CCB 4 paths.
Fig. 21 Temperature curves and regional averages of CCB 4 paths.

The study also tracked temperature changes at different stages in the 10th cycle of CCB. After filling, the mold surface heats up rapidly, and then the heat is transmitted to the mold interior and cooling channel; Spraying and blowing after removal bring further cooling. Due to the continued use of anhydrous mold release agents, the cooling at this stage is relatively mild. The retrofit effect thus comes from changes in runner flow and heat input, rather than the additional use of more aggressive spray cooling to lower temperatures, maintaining comparability with the original production method.

After simulation screening, the production mold is modified according to CCB scheme. The site was measured again with an infrared camera at the 10th cycle before spraying. Figure 22 shows that the fixed die and moving die temperatures are more uniform and the concentrated hot spots in the central injection area are reduced. The author compares the measurements and predictions again along the same paths, and the curves for each path are given in Figure 23. This two-time validation links the baseline model, modified predictions, and modified production measurements, avoiding replacing only modified model errors with modified proof of effect.

Figure 22: Measured IR temperature plot of CCB modified mold and 10 cycles.
Figure 22. Measured IR temperature plot for CCB modified mold and 10 cycles.

Visual inspection of actual castings also supports the improvement trend. Fig. 24. Two kinds of castings including runner, ingate, etc. are juxtaposed, and the flash of CCB is obviously reduced, and the burr and flash near the runner are basically eliminated. After 3000 production cycles of the modified die, the die surfaces shown do not show obvious aluminum sticking and local forming part collapse as in the baseline scheme. This observation covers a longer period of use than when the original defect occurred, providing a physical basis for the improvement of early operational stability.

Original Figure 24: Appearance comparison of CCB and original casting, including runner area.
Figure 24. Cosmetic comparison of CCB castings to the original, including the runner area.

The internal quality check selected the upper row left bracket because the baseline simulation considered it to be the most unfavorable filling condition. The total pore distribution of the control was studied along 2 sections A-A in transverse direction and B-B in longitudinal direction. In Figure 25, the predicted internal porosity region of the baseline scenario is supported by a physical examination; Cross-sections of the CCB at the same location are significantly denser and total porosity is reduced. The same part with the highest defect risk is taken as the comparison object, so that the results before and after modification have a clearer corresponding relationship.

Original Figure 25: Total porosity prediction and solid cross section comparison of upper row left stent: original scheme and CCB.
Figure 25 Prediction of total porosity of upper left stent and comparison of solid section: original protocol and CCB.

Evidence from the study included temperature paths, mold filling and porosity predictions, oxidation indices, and visual and internal cross section comparisons, showing that local runner modifications could synergistically improve mold heat balance and casting quality in this case. Among them, the die surface state of about 3000 cycles reflects the early operation performance; The original paper did not give statistics covering the entire mold life, nor did it report the exact percentage reduction in lot rejection. Quality improvement in articles is based primarily on comparative evidence at these specified locations and stages.

The author relates the extensibility of the method to the boundary condition calibration. If the new alloy is not available in the database, the heat transfer conditions between the metal and the mold need to be redefined; Thermocouples can be arranged in key parts of the mold, and parameters can be obtained according to the curve of temperature versus time. The main verification of this case is the spatial temperature distribution at a given time. The combination of these two kinds of information is helpful to further improve the applicability of the model to other thin-walled castings and different materials.

The process thread of this work is to locate hot spots and flow imbalances from production defects, compare local structural modifications with models supported by field temperatures, and finally return to field validation. the successful scheme change both that merging mode and the heat input distribution of the stream, but the scheme with only closed branches still has strong entrainment. For similar die-casting processes, runner design is therefore both a flow supply problem and a cycle heat management problem. The joint analysis of the two can explain why the local change of small size will affect the internal quality of the casting and the surface condition of the mold.

Martina Campanella、Antonio Piccininni、Gianfranco Palumbo; The International Journal of Advanced Manufacturing Technology,141,5185–5201; DOI:10.1007/s00170-025-16843-7。 This paper compiled according to the original paper, maps and data using CC BY 4.0 authorization.Original Paper · PDF · CC BY 4.0 ·