Replicating Wax Patterns with Water-Soluble Printed Molds: Dimensional Errors and Defects in Aluminum Lattice Investment Castings
Published:
2025-09-17
In this paper, water-soluble PVA negative mold was printed by FDM, then wax was injected, the mold was dissolved and aluminum alloy investment casting was performed. The four types of lattice elements and the gradually refined octet structure show that the route can reproduce complex geometries, but printing, wax shrinkage and metal solidification contribute different errors, which need to be measured and compensated step by step.
Figure 4: Wax sample after PVA dissolution and corresponding aluminum alloy casting, comparing 4 types of units and refining octet.
From Water-Soluble Printed Molds to Wax Patterns and Investment Casting
The bars and nodes of metal lattice structure are interconnected, which can form a specific spatial topology with less material, and also bring difficulties to mold manufacturing and demoulding. Direct metal printing can produce such structures, but equipment cost, forming efficiency, and surface and internal defects still need to be considered. Traditional investment casting can reproduce wax pattern details, but the manufacture of complex wax patterns may rely on specialized molds. Intrigila et al. put additive manufacturing in the previous process of wax pattern, and explored the use of ordinary FDM equipment to make one-time water-soluble female mold.
The process is not to print the plastic directly as the final baking removal pattern, but to print the negative cavity of the target lattice first, inject casting wax into it, and dissolve the external PVA with water after cooling to obtain a complete wax sample. The subsequent fabrication is still completed by wax sample treeing, embedding, dewaxing and aluminum alloy casting. In this way, the stripping of complex geometries relies primarily on material dissolution, reducing the need for mechanical stripping and manual removal of internal supports, and also restoring the dominant pattern material to casting wax for subsequent firing stages.
Four cell topologies, simple cube SC, body-centered cube BC, octet and diamond, were selected, and geometry was constructed with cylindrical members and spherical nodes. The model was generated with Boolean union in Grasshopper of Rhinoceros 3D. Due to topology differences, the relative density of elements varies even if the same basic size is used for members and nodes, and the range given in the paper is 0.17 - 0.42. In order to investigate the manufacturing boundary of finer structures, the external dimensions of octet are kept constant, and the rod diameter and node diameter are reduced step by step.

Figure 1 shows a series of structures with rod diameters gradually reduced from 2.8 mm to 0.8 mm, and the corresponding node size. This design separates two types of problems: four topologies are used to compare whether different spatial connections can be replicated, and the refinement octet is used to see what is missing when the size approaches the printing and casting limits. The forming results of this group of specific geometric and equipment conditions are studied and evaluated. Geometric scale and topology themselves participate in determining the final accuracy.
The negative mold is formed by subtracting the target structure from the cuboid surrounding the lattice, and a tapered interface is added on one side to facilitate connection with wax injection equipment. The CAD files are imported into the Ultimaker Cura slices in STL format and manufactured using the Ultimaker S5 printer. the prin material is water soluble polyvinyl alcohol PVA, and that solubility of the prin material ensures that the complex cavity does not need to be disassemble through a parting surface; The rigidity, wall thickness and internal filling of the mold need to ensure that it can withstand the subsequent wax injection load. Figure 2 shows the flow from negative form design to dissolution stripping.

The printing layer height is 0.1 mm, the outer wall uses four lines, and the inner part is filled with 50% density triangles. The extrusion temperature was 210 ℃, the platen temperature 60 ℃, and the printing speed 45 mm/s. These settings balance detail resolution with the ability of the negative mold to support. Negative horizontal expansion compensation is also applied to the outer wall and holes during slicing to offset the size deviation caused by the printed material. According to this set of settings, the printing time of 1 dot matrix negative mold is about 3 - 4 h.
| project | setting |
|---|---|
| printer | Ultimaker S5 |
| storey height, floor height, height between floors | 0.1 mm |
| Number of wall lines | 4 |
| inner filling | Triangle, 50% |
| extrusion temperature | 210 ℃ |
| platform temperature | 60 ℃ |
| printing speed | 45 mm/s |
The original paper also lists the material background for the selection of PVA: depending on the degree of hydrolysis, its melting point is about 180 - 220 ° C, its glass transition temperature is about 60 ° C, its degradation temperature is about 350 - 450 ° C, and it has strong hygroscopicity. These are the ranges of material properties used to explain its combination of printability, shape support during wax injection and subsequent solubility; The actual printing still adopts the above specific settings, and the material characteristic range and the machine process setting are recorded separately.
After printing, the molds were measured and weighed, and then the liquid wax was injected with a 1500-D.DIGIT casting wax injection device at an injection pressure of 5 - 10 bar. the PVA mold was then place in a water bath at 40. degree. C. and dissolution was facilitate by means of a vibrating platform. To maintain the dissolution process, the water was changed every 6 h until the negative mold was removed, and finally the wax sample was placed in cold water to wash the residual PVA. This process eliminates the dependence of complex structures on rigid mechanical release paths, but dissolution, cleaning, and wax shrinkage remain separate process steps.
After wax samples are obtained, wax trees are formed by connecting all the pieces to the trunk through the original wax injection connecting channels. The embedding material was Ultra-Vest MAXX gypsum-based casting material, mixed with water at 25 ℃, soaked for 1 min, stirred at 316 rpm for 4 min, and injected into the cylinder casting sleeve. Vacuum mixing equipment and vibration platform are used to evacuate air from embedded materials and reduce the chance of bubbles staying on the surface of complex lattice or in narrow positions inside. Figure 3 corresponds to the subsequent embedding, dewaxing, pouring and cleaning process.

The investment mold underwent staged heat treatment: drying at 25 ℃ for 2 h, heating to 150 ℃ over 1 h and holding for 3 h, then heating to 370 ℃ over 2 h and holding for 3 h, and finally heating to 730 ℃ over 4 h and holding for 2 h. A staged treatment is used to remove wax, drain moisture and prepare subsequent pouring conditions. The temperature program here belongs to the dewaxing and heat treatment of gypsum-based embedded type, and belongs to different processes from the extrusion and dissolution conditions of PVA in the previous stage.
| stage | Warming arrangements | incubation time |
|---|---|---|
| drying at room temperature | 25 ℃ | 2 h |
| paragraph 1 | 1 h to 150 ℃ | 3 h |
| paragraph 2 | 2 h to 370 ℃ | 3 h |
| paragraph 3 | 4 h ramp to 730 ℃ | 2 h |
EN AC 43500 (AlSi10MnMg) aluminum alloy and ASEG Galloni G5 vacuum casting equipment were used for casting. The main alloy ranges listed in Table 1 of the paper include 9.0%~ 11.5% Si, 0.40%~ 0.80% Mn, 0.10%~ 0.60% Mg, and an upper limit of 0.25% Fe. After cooling for about 6 hours after pouring, the embedded material is removed by water jet, the runner is cut off and the sample is separated. The real object is only cleaned after basic casting, no sand blasting, so a few burrs and original surface details can still be seen in the picture.
In order to distinguish the errors of each stage, PVA negative mold, wax sample after dissolution and removal of mold and final aluminum sample were observed simultaneously. The Hirox HRX-01 digital microscope is used to measure the rod diameter, node diameter and rod length, while the volume is determined by hydrostatic weighing method, and the mass is compared with the CAD theoretical value. FIG. 6 show that measurement locations and partial section. Retaining intermediate samples along the same manufacturing chain allows size changes to be attributed to printing, wax forming, and metal casting, rather than just judging accuracy by final appearance.

Dimensional Errors, Fine-Strut Limits and Shrinkage-Porosity Prediction
Figure 4 shows wax and aluminum samples of four units and refined octet side by side. The four basic topologies retain their main shapes in two stages, indicating that the water-soluble negative mold can transfer complex negative shapes to wax and then into casting. As the members become thinner, the defects begin to appear in different processes: the thinnest octet wax sample lacks some peripheral nodes and members, and another thinner wax sample can still be formed, but the peripheral nodes are missing in the metal sample. Type 2 defects point to different manufacturing processes.
The author considers that the former one is related to PVA cavity characteristics close to the size of printing nozzle and difficult to form accurately, while the latter one reflects the limitation of filling and solidification of small channels. Therefore, improving the printing resolution helps to improve the female mold, but does not automatically solve the thin rod missing at the metal end; the lat also needs to be evaluate in conjunction with metal flow, mold temperature, and runner conditions. The geometric design of the test was refined in stages to distinguish these stage limitations rather than to give a single minimum rod diameter for all lattices.
Surface observations also reveal the transmission of errors. The FDM layer by layer texture is visible on both wax and final aluminum samples, and the texture spacing measured in Figure 5 is approximately 100 μm, which is close to the slice height of 0.1 mm. The lamination of the original negative mold surface is still retained after wax injection and metal replication, indicating that geometric details can be transferred well, and that the initial printed surface will directly limit the surface quality of subsequent finished products. The back casting does not automatically remove the texture left by the front casting.

Figure 7 summarizes the quantitative results for each manufacturing stage. The rod diameter, node diameter and volume changes are compared as follows. The overall error of the inner size of PVA negative mold is about 1%~ 3%, which reflects the influence of equipment precision and material after slice compensation. The size of wax sample changes more obviously. The author summarizes that the rod diameter and node size are reduced by about 3%-7%, and the wax sample quality is about 12%-15% lower than the CAD theoretical value. There are still differences in the individual deviations of each topology in the figure, which should be read in conjunction with the data item by item, rather than regarding the generalized interval as the upper and lower limits strictly observed by each sample.
For example, the first element in Fig. 7, the rod diameter of CAD is 2.80 mm and the node diameter is 4.20 mm. the correspond values were 2.82 mm and 4.25 mm for that PVA negative, 2.58 mm and 3.96 mm for the wax sample, and 2.57 mm and 3.92 mm for the final aluminum sample. The original text gives a final rod diameter deviation of −8.22% and a nodal deviation of −6.76%. This series of data indicates that the wax sample phase has formed a large deviation, and the metal phase continues to change from the previous size.
| stage | Diameter of rod/ mm | Node diameter/ mm |
|---|---|---|
| CAD | 2.80 | 4.20 |
| PVA negative mold | 2.82 | 4.25 |
| cereus | 2.58 | 3.96 |
| metallic-like | 2.57 | 3.92 |
The final rod diameter of the remaining three basic elements in Figure 7 is approximately 2.57 - 2.59 mm, the node diameter is approximately 3.92 - 3.95 mm, and the rod diameter deviation from CAD is approximately −7.48% to −8.30%. These results show that different topologies still have different volume, mass, and local size responses under the same printing and waxing parameters. The geometric connection method changes the wax flow, gas escape and subsequent solidification conditions, and size compensation needs to be combined with specific topological judgment.
The mass variation of wax sample is larger than that of partial linear size variation, which is believed to be related to volume contraction of wax from liquid to solid state and entrained bubbles. The theoretical wax sample mass is calculated according to CAD volume and density of 0.95 g/cm ³, and the theoretical aluminum sample mass is 2.7 g/cm ³. By combining mass with independently measured volume, it is possible to determine whether contraction of shape alone is sufficient to explain mass differences; But this inference does not directly give the location, size or number of each bubble.
Compared with the average rod diameter of CAD, the diameter of the final metal sample is reduced by about 7%~ 8%, and the diameter of the node is reduced by about 6%~ 7%. The volume change of different units is more different: the volume of the first and second types of units in FIG. 7 decreases by about 7.94% and 6.74%, while the volume of the third and fourth types decreases by about 15.17% and 16.74%. The mass decreases by 12.38%, 9.88%, 15.42% and 16.73%. Therefore, the maximum volume loss of about 15%~ 17% reported in the paper mainly corresponds to the widely varying geometry, rather than a uniform result for all elements.
| in original order | volume deviation | mass deviation |
|---|---|---|
| Category 1 | −7.94% | −12.38% |
| Category 2 | −6.74% | −9.88% |
| Category 3 | −15.17% | −15.42% |
| type 4 | −16.74% | −16.73% |
From wax sample to metal sample, there are embedded dehydration and thermal expansion, metal solidification and cooling shrinkage process. The authors combine these opposite or additive variations to explain the final deviation, without attributing the total size difference entirely to the thermal contraction of the metal. In particular, some cubic structures have more obvious mass reduction than volume change, indicating that they may also contain internal pores or local voids, which need to be analyzed in combination with shrinkage conditions. Different measurement dimensions answer different questions. It is not enough to evaluate the density of the whole piece by looking at the rod diameter at one place.
Inspire Cast was used to simulate solidification and Niyama criterion was used to analyze shrinkage porosity tendency. The original formula (1) is N=G/√R, where G represents the local temperature gradient and R represents the solidification rate used in this paper. When the temperature gradient is low and the cooling speed is fast, the criterion value is low, according to which the author identifies the unfavorable region of shrinkage. N=0.30 is used as the discrimination threshold for the aluminum alloy used in this study. Figure 8 shows the prediction distribution of 4 kinds of units.

There are many areas below the threshold in the simulation, which is consistent with the researchers 'judgment of shrinkage risk, and also provides a mechanism explanation for the final volume and mass lower than CAD expectations. This part is based on thermal analysis and empirical criteria of defect prediction, and the microscope to measure the rod diameter, weighing the quality of the different evidence. The original paper did not provide point-by-point verification of each low-N region corresponding to a tomographic pore, so predictions were mainly used to interpret trends and determine the direction of subsequent optimization.
This study kept the runner system unchanged, and did not complete the comparison between the old and new feeding schemes in the same test. The authors suggest that sprue, riser and exhaust can be redesigned according to simulation, preheating and cooling conditions of mold can be adjusted to reduce the risk of defects at joints and near thin rods. Lattice has both small channels and local thick nodes, and flow and solidification restrict each other. Therefore, further improvement needs to take care of both wax pattern replication accuracy and metal shrinkage, not just reduce the print height.
In wax pattern design, the possibility of reverse compensation is discussed: scaling or local deformation of the negative pattern geometry according to the measured phase shrinkage, and then checking whether the final deviation is reduced. In the current data, the direction of printing error and wax sample deviation is not always consistent, and the change of node, rod diameter and volume is not completely in the same proportion. It can be seen that although a single overall magnification factor is easy to implement, whether it is sufficient still needs to be judged by repeated measurements combined with local characteristics.
The direct result of this work is to verify the process connectivity of water-soluble negative printing-wax injection-metal casting and to reveal how errors gradually accumulate. The data of about 3 - 4 h corresponds to the printing time of a single PVA negative mold only, and the complete manufacturing cycle also includes wax injection, dissolution, embedding, heat treatment and cooling. The original paper also did not give a complete batch cost or lattice mechanical properties of the control test, so its "rapid prototyping, low volume manufacturing" potential is mainly based on the feasibility of the process and reduce the dependence on special tooling.
For complex lattice castings, this study provides an evaluation method that can be traced step by step: first check whether the negative mold is formed according to CAD, then measure the wax pattern size and quality, and finally relate the local size, total volume and solidification prediction of the metal sample. The solubility of PVA solves the problem of obtaining complex wax samples; Shrinkage, surface texturing and thin rod filling still require their own process optimization. Keep this chain of evidence to judge whether the next round of improvement should be prioritized in printing, wax injection or casting.
Claudio Intrigila、Daniele Almonti、Silvio Genna、Paolo Bisegna、Vincenzo Tagliaferri; The International Journal of Advanced Manufacturing Technology,140,4033–4043; DOI:10.1007/s00170-025-16455-1。 This paper compiled according to the original paper, maps and data using CC BY 4.0 authorization.Original Paper · PDF · CC BY 4.0 ·
Related News