Thick-Walled Steel Castings: Microstructure and Impact Properties across a G17Mn5 Ladle Wall


Published: 

2025-08-19

The wall thickness of G17Mn5 cast steel slag pot was sampled along the decommissioning line. Combined with composition, inclusion, impact and micro-tensile tests, how the center segregation and inner wall cracks deteriorate the local toughness before the overall strength was analyzed.

Figure 2 of the original paper: Crack network exposed after grinding on the 8th plate of the inner wall.

Figure 2 of the original paper: Crack network exposed after grinding on the 8th plate of the inner wall.

Sampling along the wall thickness, the composition, structure and mechanical test

The outer wall, center and inner wall of large steel castings undergo different solidification and service thermal histories. Segregation, inclusion aggregation and local toughness deficiency may exist in thick wall even if some average strength requirements are met in the same furnace. Kalandyk et al. studied a retired slag pot. The purpose was not to judge the whole material by a set of tensile results, but to establish a correspondence between composition, structure, impact absorption energy and micro-tensile along the wall thickness and observe how the most unfavorable areas were formed.

The slag ladle is made of G17Mn5 low carbon cast steel with a capacity of 16 ‰ 18 m³. The sampling position is located above the side wall of the tank body close to the bottom, and the local wall thickness is about 0.13 m. This type of slag pot usually requires a yield strength of more than 205 MPa, a tensile strength of about 405 - 600 MPa, and an elongation of more than 24%. These are material requirements in the context of the study and are not acceptance conclusions for this decommissioned slag pot after testing has been completed. In actual service, slag pot repeatedly contacts high temperature slag and is transported outdoors. Thermal cycle and seasonal temperature difference will affect the material.

The specimen was divided into 8 cuboid plates of approximately equal thickness, each about 13 mm thick, and numbered progressively from the outside to the inside. The 8th plate, the innermost surface, was exposed to the crack network during grinding and therefore did not enter the main seven plate performance control. Plates 1 - 7 were used for impact and tissue testing, respectively, and tensile microspecimens were prepared from selected plates. In this way, the inner wall layer with obvious cracks can be distinguished from the rest of the region, avoiding mixing the samples with irregular failures directly into an average value.

Figure 1: Sampling position and plate number from outside to inside along slag pot wall thickness.
Fig. 1 Sampling position and plate number from outside to inside along slag pot wall thickness.

Chemical composition was determined using SPECTROMAXX spectrometer, the outer, central and inner regions of wall thickness were examined separately. Total oxygen was measured using a LECO RO16 analyzer. Metallographic structure was observed by Leica optical microscope and JEOL scanning electron microscope, and inclusion composition was examined by EDS. Non-metallic inclusions were measured using Keyence optical systems and each sample was analyzed at 400x magnification over an area of 6.3 mm². The microstructure and composition data are thus not borrowed from another slag pot, but correspond directly to the current wall thickness position.

The impact test was performed using a 300 J pendulum, and specimens of 10×10×55 mm with a V-notch depth of 2 mm were prepared in accordance with ISO 148-1:2010. Temperatures of +20 ℃, 0 ℃, and −10 ℃ correspond to the environmental changes that may be experienced from summer to winter. The test compares the impact absorption energy at the specified notch and temperature, with the unit being J, which should not be mixed with the tensile strength MPa, nor should the room temperature results be directly used for brittle fracture judgment in low temperature environments.

Hardness is measured along the cross-section at 4 locations per plate using carbide balls of 2.5 mm diameter, a test force of 187.5 kgf and a holding time of 15 s. The results were compared according to their labeled HBW values. Hardness can reflect local structural changes, but it is not the same index as toughness: pearlite increase may make the center harder, but at the same time reduce the impact bearing capacity. Therefore, the author did not take the higher hardness as the basis for better performance in this area.

The microtensile specimen is further processed from the macroimpact specimen material. Based on previous metallographic, hardness and impact results, the authors selected plates 1, 2, 4, 5 and 7 for static tensile testing. Firstly, strip material with thickness of about 1 mm is cut, and then micro-sample shape is obtained by wire cutting; The spacing between adjacent strips is approximately 0.32 mm, and the spacing between adjacent work sites within a strip is approximately 1.32 mm. Wire cutting uses 0.25 mm CuZn37 brass wire, current 4.5 A, voltage 80 V, and prolong pulse interval to minimize the effect of processing heat on tissue.

Figure 3: Path and size of microtensile specimens cut from macrospecimens.
Fig. 3 Path and size of microtensile specimen cut from macrospecimen.

The loading device is MFS micro-fatigue test system. The load is applied by actuator displacement. The positioning accuracy of nano-actuator is 1.7 nm, and that of micro-actuator is 1 μm. Because the gauge length area is very small, the deformation is measured by using the digital image correlation DIC method, and the natural texture of the surface is directly utilized, and no speckle mark is additionally made. Telecentric lenses and high-resolution cameras are used to observe local deformations. The positioning accuracy here is used to describe the ability of the test system and cannot be directly interpreted as the deformation measurement accuracy of the whole slag pot.

How Segregation, Inclusion, and Crack Change Strength and Toughness

Ferrite is dominant with pearlite islands in the outer and inner regions. The pearlite proportion is higher in the central region. Spectrum analysis showed that the carbon content in the center increased to about 0.25%, and the outer and inner regions were about 0.19% and 0.20% respectively. Sulfur is also concentrated in the center, about 0.03%, and in the outer and inner regions, about 0.014%-0.015%. The author discusses this distribution together with solidification segregation and service thermal cycle of thick walled parts, but does not give a continuous record of point-by-point composition before and after service at the same position, so all differences cannot be attributed to service diffusion alone.

C and S distribution along wall thickness
locationCarbon/%Sulfur/%
outside0.190.014–0.015
centre0.250.03
inside0.200.014–0.015

The spatial difference in total oxygen was not significant, with measurements ranging from 137 - 160 ppm, above the recommended level of about 40 - 60 ppm discussed in this article. Nonmetallic inclusions exist in different regions, and oxygen-sulfur inclusions are irregular in shape. From the 3rd and 4th plates in the center to the 7th plate in the inner side, type Ⅱ MnS can also be seen along the original grain boundary. It is believed that sulfur segregation is beneficial to this kind of precipitation, and its dendritic and slender distribution makes it easy to form local stress concentration between inclusions. The inclusion volume fraction of the 4th and 5th plates is higher, which corresponds to the unfavorable microstructure characteristics of the center and adjacent areas.

Figure 7: Nonmetallic inclusion morphology at different wall thickness locations.
Fig. 7 morphology of nonmetallic inclusions at different wall thickness positions.

Table 2 lists the inclusion volume fraction along with the size distribution. The volume fraction of plate 1 - 7 was 0.26%, 0.20%, 0.22%, 0.30%, 0.60%, 0.20%, 0.20% respectively. The fifth plate has the highest total volume fraction, and the inclusion count larger than 100 μ m is 118; The fourth plate corresponds to a count of 44 and the first plate to 28. These measurements are from fixed observation areas and indicate that the number of inclusions between zones differs from the size composition and is not the total number of inclusions for the entire slag pot. Central carbon segregation, inclusion morphology and inner cracks need to be analyzed jointly, and all impact low values cannot be explained only by the location of the highest volume fraction.

When the proportion of central pearlite increases, the hardness reaches about 138 HBW, which is summarized as about 140 HBW in the conclusion of this paper. Other areas are mainly 125 - 130 HBW. Compared with the average normalized hardness of 156 HBW of the pre-service specimens, the hardness of the retired specimens is about 20 ‰ 30 HBW lower. However, the quality, wall thickness and solidification rate of the casting specimen are different from those of the bulk specimen. The author also considers these differences and macrosegregation of carbon as possible causes. This is not a comparison of the same piece of material under exactly the same conditions, and the hardness difference cannot be directly regarded as the service degradation amount.

Figure 10: Hardness variation measured along slag pot wall thickness.
Fig. 10 Hardness variation measured along slag-pot wall thickness.

The impact results reveal local weak areas more clearly than tensile strength. At +20 ℃, the first and second plates on the outer surface absorb about 42 - 53 J of energy; The fourth plate in the center is about 24 J, which is lower than the minimum requirement of 27 J used in this paper. Plate 5 - 7 is about 28 - 30 J, although it is still slightly higher than this value in similar microstructures, but it is significantly lower than that in the lateral side. The abstract and detailed results indicate that the center is about 24 J, and the judgment should be based on this specific position data, and the whole wall thickness cannot be generalized as qualified at room temperature.

Figure 11: Charpy impact absorbed energy for various panels at different temperatures.
Fig. 11 Charpy impact absorbed energy of each plate at different temperatures.

When the temperature was reduced to 0 °C, the impact absorption energy of each region is further reduced. The conclusion of the original text shows that the second to seventh plates do not exceed 20 J, and the first plate is about 22 J, which is lower than 27 J. At −10 ° C, this requirement is also lower. Therefore, examination of only one outer wall sample at +20 ℃ would mask the central weak zone and would not reflect the increased brittleness at low temperature transport. The three temperatures used in the paper provide this trend, but are not sufficient alone to draw a complete ductile-brittle transition curve or determine critical points at all service temperatures.

Fracture analysis shows that the low impact energy corresponds to the mixed mode fracture, and the central region is dominated by brittle cleavage planes with microcracks. The change of cleavage direction, step and less shear lip support the judgment that brittle failure occurs obviously. Combined with energy spectrum, the authors observed dense type Ⅱ MnS on the fracture surfaces of plate 4 and plate 7, some of which had dendritic morphology. Inclusion composition, morphology and spatial distribution need to be evaluated together, and total sulfur content or a low-magnification photo cannot replace fracture evidence.

Fig. 13: Inclusion aggregation and composition observation in fracture.
Fig. 13 Inclusion aggregation and composition observation in fracture.

Plate 8, which was excluded from the primary control, still had independent observation value. The crack network on the inner wall extends into the interior of the material, and the impact absorption energy reported separately is 6.8 - 29 J, which is very discrete; Some of the specimens did not crack from the specified notch. This indicates that existing cracks can alter the crack path and failure location, so this set of results cannot be combined directly with the normal notch test of plates 1 - 7 to find an average impact value that seems to represent the entire slag pot.

Tensile testing gives another control. The stress-strain curves of the 1st and 2nd plates are close to coincidence and have good repeatability. The strength characteristic value of the fourth plate in the center is higher, but the dispersion is more obvious, and the tensile strength deviation reaches 30.5 MPa. The author relates the strength increase to carbon enrichment and pearlite increase, and considers that dendritic sulfide inclusions will increase the differences between microsamples. It can be seen that higher local strength and poor impact toughness can occur simultaneously, and they are not contradictory.

Original Figure 16: Tensile stress-strain curves of micro-specimens with different wall thicknesses.
Fig. 16 tensile stress-strain curves of micro-specimens with different wall thicknesses.

The tensile curves of the 5th and 7th plates are more irregular, some curves suddenly drop, and the elongation after fracture is lower and more dispersed. The authors believe that this may be related to the combined action of microcracks and nonmetallic inclusions: when the local stress reaches a critical level, the discontinuity propagates rapidly, resulting in a sudden decrease in load bearing capacity. In contrast, the difference in the wall thickness direction between the yield strength and the tensile strength is less pronounced than the difference in the impact absorption energy and the elongation. Checking only conventional strength values may miss toughness issues that affect safe decommissioning judgments.

Figure 17: Comparison of average mechanical properties of panels with different wall thicknesses.
Fig. 17 Comparison of average mechanical properties of plates with different wall thicknesses.
Excerpt from original Table 3: Average mechanical properties of micro-specimens (mean ± deviation from original table)
PlateUTS / MPaYS / MPaEL / %
1397 ± 2222 ± 027 ± 1.5
2397 ± 2.5222 ± 324 ± 1
4434 ± 30.5232 ± 725 ± 1
5427 ± 20238 ± 8.520 ± 5.5
7391 ± 15224 ± 623 ± 6.5

Table 3 shows that the average tensile strength of plates 1, 2, 4, 5 and 7 is 397±2, 397±2.5, 434±30.5, 427±20 and 391±15 MPa respectively; The corresponding yield strengths were 222±0, 222±3, 232±7, 238±8.5, and 224±6 MPa. Although the fourth plate in the center has higher strength, it is the most unfavorable position for impact performance. The average yield strength of the fifth plate reaches 238 MPa, which can not exclude the problem of large scatter in elongation. The mean and deviation are expressed in the original table and are not further interpreted as intervals with specified confidence levels.

The mean and dispersion of elongation were 27±1.5% in the first plate, 24±1% in the second plate, 25±1% in the fourth plate, 20±5.5% in the fifth plate and 23±6.5% in the seventh plate. The dispersion of the 5th and 7th plates is obviously larger than that of the 1st and 2nd plates, and the irregular decrease in the corresponding curve indicates that the influence of local discontinuity in small size samples cannot be ignored. Micro-sample is used in this paper to correspond to wall thickness partition, which is not exactly the same as macro-sample size and sampling conditions in material standard, so micro-sample results cannot unconditionally replace product standard tensile acceptance.

The results of this paper fall into metallurgical quality control of large thick-walled steel castings: refining and modification after melting are helpful to reduce the volume fraction of inclusions, adjust the morphology and distribution of inclusions, and solidification cooling conditions affect the segregation of thick sections. It is suggested that sulfur and phosphorus should be controlled especially for important large castings, and the limit value given in the discussion should not exceed 0.02%. This proposal is a process discussion for thick wall castings and does not replace the requirements of specific product drawings, material standards and service conditions.

The practical implication of the study is to map the detection location to the service area. The outer wall sample, center sample and inner wall crack layer represent different states, and the structure, composition, hardness, impact and micro-tension need to form evidence of mutual support. The results of the decommissioned slag pot reveal the path that segregation, inclusions and thermal fatigue crack weaken local toughness together. Since there is no complete pre-service and post-service tracking of the same part and no full load history is given, it is more appropriate for the data to be used to explain the risk mechanism of this piece and similar thick-walled steel castings, and it is not possible to calculate the unified residual life of all slag ladles.

Barbara Elč bieta Kalandyk, Dariusz Boroński, Paweč Maćkowiak, etc.; Materials 18(16), 3877; DOI:10.3390/ma18163877。 According to the original paper, the drawings and data are authorized by CC BY 4.0.Original Paper · PDF · CC BY 4.0 ·