Sintered Bauxite Sand for 3D-Printed Cores: Recoating Speed, Strength and Pump-Housing Casting


Published: 

2025-07-07

Sintered bauxite sand and quartz sand were compared on the same VX500 equipment, sand spreading, furan resin and acid catalyst were investigated, and the forming and cleaning performance of aluminum alloy pump housing were verified by trial casting.

Figure 13: Sintered sand core, pump housing trial casting and observation of sand inclusion on the contact surface of two kinds of sand core.

Figure 13: Sintered sand core, pump housing trial casting and observation of sand inclusion on the contact surface of two kinds of sand core.

From particle characteristics to recoating, bonding and performance evaluation

The printing material of sand core cannot be selected only according to fire resistance. Particle shape and particle size determine whether the powder can be evenly spread, resin and catalyst determine the handling strength after curing, and permeability, surface roughness and sand cleaning difficulty will affect the casting. Erhard et al.'s study places these steps in the same process chain: parameters of sintered bauxite sand are established on commercial binder injection equipment, then compared with common quartz sand, and finally aluminum alloy pump housings with complex cavities are cast.

voxeljet VX500 was used in the experiment. The plane size of the working box was 500 × 400 mm, the maximum depth was 300 mm, and the nozzle resolution was 360 dpi. The sand spreader releases particles through slits under vibration and is smoothed by scrapers. The recoating direction is perpendicular to the nozzle scanning direction. By fixing the spray conditions such as nozzle waveform and changing the amount of adhesive deposited per unit area through periodic pixel patterns, the author avoids mixing the variation of nozzle driving energy with material curing effect. Figure 1 shows sample arrangements and how different pixel densities can be achieved.

Figure 1: Sample layout and pixel patterns of different adhesives in the VX500 workbox.
Figure 1. Sample layout and pixel pattern of different adhesives in VX500 workbox.

The sintered sand CastBall AFS 65 Premium 3D is made by grinding, pelletizing and sintering at high temperature. The main crystalline phase is corundum, and the silicon enters mullite or other amorphous phases. According to this, it is pointed out that the material does not contain free crystalline silica. The control material was GS14RP quartz sand. The average particle size given by the supplier is approximately 0.21 mm and 0.13 mm respectively. The sphericity and roundness of sintered sand are higher, and the particle size distribution is narrower. These features facilitate flow, but coarser particles may also roughen the profile.

Differences in material density affect the comparison of formulations. Table 1 lists sintered sand bulk density of 2.12 g/cm³, particle density of 3.73 g/cm³, quartz sand corresponding to 1.32 and 2.65 g/cm³. Even if the resin mass percentage of the two is different, it does not necessarily mean that the deposition conditions of the printhead are different. Therefore, the binder dosage was divided into low, medium and high relative levels: 2/3, 1, 4/3. The medium level corresponds to 2% of the mass of quartz sand and about 1.42% for sintered sand with higher density. Comparisons should be made while retaining relative deposition levels and content by sand mass.

Excerpt from Table 1: Density and 600 ℃ Thermophysical Properties of Sand Materials
parametersinter bauxite sandsilica sand
Bulk density / g·cm⁻³2.121.32
Particle density / g·cm⁻³3.732.65
Thermal expansion/ %0.0191.2
Specific heat capacity / J·g⁻¹·K⁻¹0.4601.25
Thermal conductivity / W·m⁻¹·K⁻¹0.4070.345

Table 1 also lists thermal properties at 600 ℃: thermal expansion of sintered sand is about 0.019%, quartz sand is about 1.2%; Specific heat capacities are about 0.460 and 1.25 J/(g·K), respectively, and thermal conductivities are about 0.407 and 0.345 W/(m·K), respectively. These data are used to explain the difference of sand species itself, and are not direct measurements of the temperature field inside the pump housing. Low thermal expansion helps reduce the change in core size with temperature, but the hot cracking, veining or metal penetration of specific castings are still affected by the combination of pouring, structural constraints and bonding systems.

Both sands are stored at room temperature without additional sieving and mixed with p-toluenesulfonic acid-based catalyst prior to printing. The main component of the spray binder is furfuryl alcohol, which is RPT2 system. The catalyst content of sintered sand was set at 0.2%, 0.3%, 0.4%, and the recoating speed was set at 100, 200, 400 mm/s. 0.2% catalyst and 100 mm/s recoating speed were used for quartz sand. Layer thickness is 0.28 mm, bake-free curing system is used, and the samples are printed and placed for 24 h under ambient conditions before characterization or casting.

Particle characterization using PartAn 3D optical particle analyzer. Take care of fine particles and coarse particles, and let the whole sample pass through the instrument to avoid missing the fine powder when it is concentrated in the later stage. Particle size statistics are expressed as relative, cumulative mass fractions on a sieve, while shape parameters are normalized to 0 - 1, where 1 represents ideal sphericity. Micrographs and particle size analysis results are consistent. According to the definition of passing through a 230-mesh sieve, the fine powder content of sintered sand is about 0.2%, and that of control quartz sand is about 0.5%.

Figure 3: Comparison of particle size distributions of sintered bauxite sand and quartz sand.
Fig. 3 Comparison of particle size distribution between sintered bauxite sand and quartz sand.

Three point bending was used for the primary mechanical evaluation. Test strip section 22.4 × 22.4 mm, length 172 mm, support span 150 mm, test machine equipped with 20 kN sensor; Each group is usually tested with 5 pieces, and the actual effective quantity in some figures is 4 ‑ 5 pieces. The authors also compared the wear resistance with Simpson scratch hardness tester, measured at the same position on the side end of the test strip. The instrument gives dimensionless B scale, the value is used for comparison between the test materials, and should not be directly converted to the life of other wear tests.

Air permeability is measured according to BDG P41 and AFS 5224 - 13-S correlation method, and the sample is a cylinder with a diameter of 50 mm and a height of 50 mm. Surface quality is measured using an SJ-410 instrument, with emphasis on reporting the average roughness depth Rz, measured in a plane perpendicular to the build direction. The roughness of the contact surface between the mold surface and the corresponding aluminum casting is evaluated by the same method, so that the effect of material particles on the mold and casting surface can be analyzed together.

Parameter Coupling, Pump Housing Trial Casting and Material Selection

The good fluidity of sintered sand makes it possible to lay sand at 400 mm/s; When the same equipment processes GS14RP quartz sand, visible macro ply defects appear when the speed exceeds 100 mm/s. However, the maximum paving speed is not equal to the maximum bending strength. A comparison of 100 - 400 mm/s for 0.3% catalyst fixation shows that the better average strength is obtained at 200 mm/s for all three binder levels. The medium binder level is about 2.3 MPa, and the gain is about 2.5 MPa after increasing 1/3 of the deposition amount. The gain is not proportional to the amount.

Figure 6: Three-point bending strength for different recoating speeds and binder levels.
Fig. 6 Three-point bending strength at different recoating speeds and binder levels.

Catalyst and binder need to match. In Figure 7, at 0.2% catalyst, the strength of low binder level is about 0.9 MPa, but it is about 0.5 MPa and 0.4 MPa after increasing to medium and high levels. When catalyst is insufficient, adding resin does not guarantee the increase of effective bonding bridge. When the catalyst content increased to 0.3%, the binder content increased, and the positive contribution was observed. When 0.4% catalyst and high binder were used, the average bending strength reached about 3 MPa. This result shows that directly copying the resin formula of quartz sand may wrongly judge that the new sand is not suitable for printing.

Figure 7: Catalyst and binder levels together affect sintered sand specimen strength.
Fig. 7 Catalyst and binder levels together affect the strength of sintered sand specimens.

The explanation given in this paper is related to the acidity and basicity of materials. The pH of the sintered sand without additives is about 7.1, and the reference value of the quartz sand is about 6.3. The sintered sand requires more acid catalyst to form the proper curing conditions with the deposited furfuryl alcohol resin than the more acidic quartz sand. However, with the increase of liquid addition, the original fluidity will be weakened through the liquid bridge between particles. When 0.4% catalyst is added, sintered sand can still form samples without obvious lamination defects at 200 mm/s. Continue to increase the amount, it may still encounter agglomeration and uneven powder spreading.

From the point of view of process evaluation, fluidity, strength and forming accuracy are not combined into a general score, but their changes are observed separately. The time of layer deposition was shortened with the increase of recoating speed, but resin deposition was still restricted by the scanning mode of nozzle. Similarly, higher room temperature flexural strength does not directly predict post-casting cleaning time. Different indexes of samples and measurement methods are different, when selecting production formula, it is necessary to first clarify the minimum requirements of complex sand core in core assembly, handling and casting, and then judge whether increasing resin and acid content brings sufficient benefits.

The author printed the same parameters for the second time. Figure 9 reflects that there are obvious differences between batches in bending strength of two kinds of sand. Although nozzle droplet quality is checked each time, uniformity of catalyst mixing, statistical distribution of localized layup defects, and temperature and humidity during printing and curing may affect results. The absolute dispersion of high intensity group is larger, which does not mean that its relative fluctuation is necessarily worse. The paper therefore retains duplicate batches rather than reporting only the highest intensity, and subsequent scale-up production still requires larger samples to establish process stability.

When sintered sand with 0.4% catalyst and 200 mm/s is compared with quartz sand with 0.2% catalyst and 100 mm/s, the scratch wear resistance values at standard binder level are about 43 and 20 respectively. The higher values suggest that the sintered sand specimens are less susceptible to abrasion during handling, but are not a direct life test for molten metal scour. Figure 10: There are only 2 samples in each group, and the evidence range shall be consistent with the specific test method.

Figure 10: Comparison of scratch abrasion resistance values of two printing sand materials.
Figure 10 Comparison of scratch wear resistance values of two printing sand materials.

The average permeability of sintered sand is about 315 and quartz sand is about 224. In this series of trials, the adhesive level did not show a decisive effect. The authors attribute the difference mainly to particle size, and suggest that rounder particles may also improve gas passage. The numerical value here belongs to the permeability index of the instrument and method used, and cannot be directly regarded as the exhaust flow rate of the actual pump housing, nor can it be independently proved that the porosity defect must be reduced.

Figure 11: Comparison of air permeability of two printing sand materials.
Fig. 11 Comparison of air permeability of two printing sand materials.

Coarse particles carry a cost in surface quality. The Rz of sintered sand is about 170 μm, and that of quartz sand is about 104 μm. The change of Rz with the amount of binder is small. The sand mold profile affects the casting surface, but the Rz of metal castings is usually lower than that of the corresponding profile due to wetting, etc. This trend is obtained in the same measurement direction, but the influence of printing direction on roughness is not expanded into independent variables, so the results cannot be directly extended to all tilt angles and all cavity positions.

Figure 12: Comparison of Rz roughness between printed profiles and aluminum castings.
Figure 12 Rz roughness comparison of printed profiles versus aluminum castings.

3D Benchy model is used for geometric verification, and the chimney hole of about 3mm is still formed under the condition of coarse sand. The cores made of the two kinds of sand were put into GS14 RP printing sand mold respectively, and AlSi7Mg0.3 aluminum alloy was poured at 750 ℃. The diameter of the internal disk structure of the casting is about 180 mm, and the thinnest part is about 8 mm. although that sinter sand core has higher room-temperature strength, the sinter sand core is slightly easy to remove after pouring; The average Rz measured on the inner surface of the pump casing is about 108 μm, which is basically consistent with the measurement result of the flat casting.

The ease of sand removal does not mean that all surface defects are improved simultaneously. Sand inclusions were observed on the surface of castings contacting sintered sand and quartz sand castings. The author discusses two possibilities: coarser particles have larger spacing and are easily enclosed by metals; It is also possible that the sharp edges of the support scrape sand during core assembly, which in combination with vertical parting and gating system design causes inclusions. Due to the darker color of the sintered sand, inclusions may also be more noticeable. These possibilities are not divided into single reasons which have been proved in the paper, and they still need to be verified by core support and liquid metal erosion test.

The author also pointed out that sintered sand may be separated from other molding materials by magnetism, but this time a complete recovery line has not been established, and the particle size, fine powder and strength changes after repeated reuse have not been quantified. No free crystalline silicon in the raw sand, abrasive particles, and thermal decomposition emissions of acid-catalyzed furan system are material and process problems at different levels. To compare the overall environmental benefits, energy consumption of sintered raw sand, printing material utilization, post-casting recycling and actual emissions still need to be placed in a unified life cycle boundary. Individual material characteristics alone cannot be used to declare that the formulation has achieved lower total emissions.

Material selection ultimately requires consideration of tact time, core strength, sand removal and cost. The parameter of 200 mm/s established in this paper can double the speed of sand laying stage compared with 100 mm/s of quartz sand, but it can not be claimed that the whole manufacturing cycle can be halved. The raw material cost of sintered sand is estimated to be 5 - 10 times of quartz sand, and the number of recycling times will obviously affect the actual cost; high acid catalyst usage also changes that emission burden. Inorganic bonding systems such as sodium silicate are listed as follow-up directions by the authors, rather than alternative formulations that have been validated this time. Testing of the pump casing supports the feasibility of this material process route, and the mass production decision still needs to be combined with the overall verification of reuse, emissions, and casting quality.

Patricia Erhard, Carla Reddersen, Lucas van den Bosch, Daniel Günther, etc.; International Journal of Metalcasting; DOI:10.1007/s40962-025-01691-8。 Figures and data according to original paper, CC BY 4.0.Original Paper · PDF · CC BY 4.0 ·