From Furan-Bonded Printed Sand to High-Temperature Casting Molds: Impregnation, Sintering and an Impeller Trial
Published:
2025-03-15
Solid proppant and hollow cenosphere sands form different mold components. Silica-sol impregnation and sintering replace the organic bond, with microscopy, bending tests, shrinkage measurements and a nickel-alloy impeller trial evaluating the resulting mold.
Figure 17: Ni-base alloy impeller trial casting, flash and penetration phenomenon and geometric deviation diagram.
Two Sands and the Impregnation–Sintering Route
Binder spray sand mold can directly form complex cavity, but common furan resin system into superalloy casting, will encounter different problems from ordinary sand mold. The resin releases gas when it is decomposed by heat, and the strength of the mold decreases with the disappearance of organic bonds. If the as-printed sand mold is directly used for processes requiring higher preheating temperatures, only the forming accuracy is not enough to ensure subsequent casting. The method studied in this paper is to use furan resin to complete printing and handling, then immerse in silica sol, and establish inorganic bonding bridge after heat treatment.
this route separate that geometric fabrication from the final heat resistant bonding. The printing stage still uses relatively mature jetting equipment and resin system, the infiltration stage makes colloidal silica enter the particle gap, the original resin is burned during sintering, and the inorganic components assume the subsequent bonding effect. The author did not only make a model that could be displayed, but first compared the structure, strength and shrinkage of the sample, and then applied the selected process to the actual nickel-base superalloy impeller to check what problems would occur in the assembly of the model and the casting surface.
Raw sand is divided into two categories. ID50-K proppant proppant sand is composed mainly of alumina and its particles are nearly spherical. It is intended to be used to directly form cavity parts of castings. Another kind is light hollow cenosphere sand, mainly containing mullite and glassy components, intended to form the upper part of the sprue cup and riser. The choice of the two materials was intended to take advantage of the different density and heat transfer characteristics to obtain different cooling processes for the casting and the feed zone, rather than to assume that the same material must be used at all locations throughout the mold set.
The printing equipment was SP500, using DF-400 furan resin, DFG-30A acid curing agent and MH 2820 piezoelectric jet head, and the droplet volume was about 40 pL. The resolution of proppant sand and cenosphere sand are 1370×150 dpi and 1370×300 dpi, respectively, and the thickness of layer is 0.4 mm and 0.3 mm, respectively. The proportion of premixed acid curing agent is 0.5 wt.% and 4 wt.% respectively. The two kinds of sand have different particle size and specific surface area, so it is impossible to duplicate the same set of blasting and mixing parameters.
After printing, the samples were placed in the forming cavity for 24 h, and then the unbonded sand was removed with a brush. Structural analysis, thermogravimetric and bending specimen size 40×20×8 mm, flat orientation, 8 mm thickness along the Z axis of the printing platform movement. Strip shrinkage specimen is 163 x 10 x 10 mm, also USES the flat direction. thus, in subsequent comparison, that orientation of the samples remain the same, and no change in layer orientation is mixed into the effect of the number of impregnation.
The impregnation medium is UltraCast One+ silica sol, silica solids content 25.5 - 27.5 wt.%, colloidal particle size 8 - 10 nm. The sample is immersed completely for 1 min each time, and dried in air at room temperature for 24 h after being taken out; The furnace is heated at 10 - 20 ° C/min and then cooled with the furnace. Figure 1 shows the complete processing sequence. Scheme Ⅰ adopts twice infiltration followed by sintering, Scheme Ⅱ increases the infiltration of proppant sand to three times; Scheme III for cenosphere sand is to add intermediate heat treatment after the first two infiltrations, then two infiltrations and final sintering.
The temperature in Figure 1 is just as important as the holding time. The final sintering of the three schemes is 1200 ℃ for 4 h, the intermediate treatment of scheme Ⅲ is 600 ℃ for 2 h, and the impregnation before and after are combined with 24 h room temperature drying. We cannot simplify "heat treatment before infiltration" into putting the wet mold directly into the high temperature furnace, nor can we omit the step of reintroducing inorganic binder after removing resin in the middle, otherwise the comparison is no longer the scheme established in this paper.

The choice of this combination process is also related to the choice of other ceramic additive manufacturing routes. The photocuring method of pastes reviewed by the authors can form complex details, but some materials and sintering systems exhibit higher linear shrinkage, and different printing directions may be different; Reducing the sintering temperature, while helping to reduce shrinkage, reduces strength. For cast shells, the goal is not to achieve the highest strength of structural ceramics, and excessive restraint may increase the risk of hot cracking. The key is to maintain shape and process operation with sufficient post-fire strength.
The difference between these options is not just "one more dip." If the organic resin still occupies the space between particles, the pores into which the new silica sol can enter are limited; Removal of resin by intermediate heat treatment followed by impregnation may cause inorganic binders to enter the previously occupied sites. Therefore, the thermogravimetric weight loss, phase and fracture structure were observed simultaneously, instead of deducing the whole process only by the final bending strength.
SDT Q600 is used for thermogravimetric analysis, air is used as carrier gas at 100 mL/min, 20 - 90 mg sample is placed into corundum crucible, and the temperature is increased from 20 ℃ to 800 ℃ at a heating rate of 10 ℃/min. The sensitivity of mass change of the equipment is 0.1 μg. The measurement errors of mass and temperature are ±1% and ±0.5 ℃ respectively. This set of tests is used to determine the temperature range in which the organic components mainly leave the mold, and to provide a basis for the selection of intermediate heat treatment temperature.
Particle morphology, fracture surfaces and elemental distributions were examined by SEM and EDS; ImageJ measured particle size and shape, and Cu Kα XRD identified phases. Three-point bending used an Instron 5966 according to ASTM C1161-13, with a 21 mm support span and 1 mm/min loading rate. A caliper with ±0.05 mm error measured long specimens before and after sintering. Original Equation (1) is ε = (L₀ − L) / L₀ × 100%, where L₀ is the as-printed length and L the length after final sintering.
In order to observe the interior and not limit to fractures, the authors also used micro-CT. A representative columnar sample with a diameter of 5 mm reaches a voxel size of 6. m u. m, and a 20×20×10 mm sample uses a voxel of 15. m Voltage 70 kV, current 50 μA, exposure 2 s, data collected for 1440 rotations, no averaging or pixel binning. After reconstruction, the raw sand, binder and porosity were sectioned, and Figure 2 shows the sectioning and sectioning of the proppant sand specimen.

The actual mold consists of three parts with a wall thickness of about 10 mm. The upper part No. 1 contains a sprue cup and serves as a riser, using cenosphere sand; No. 2 and No. 3 parts form impeller cavity, using proppant sand. Ceramsite sand component selection scheme II, cenosphere sand component selection scheme III. Because the intact mold is larger than the sample, each infiltration is extended from 1 min to 5 min. Figure 3 also shows the impeller, gating system and block relationships that relate the sample material evaluation to the mold that really needs to be assembled.

Before final sintering, the molded parts are placed in steel containers with coarse corundum sand as support. Before casting, the sand mold together with the supporting sand is preheated to 800 DEG C; 4 kg Ni-base superalloy was melted in magnesia crucible of induction furnace, and the melt was protected by air environment and silicate glass slag, and poured into sand mold at about 1500 ℃. Although the paper discusses the requirements of high temperature and vacuum casting on materials, this impeller verification itself uses air melting conditions, and the two need to be distinguished in the process records.
Casting evaluation includes both surface and geometric components. Confocal microscopy measures the surface roughness Sz in the area of 1.2×1.2 mm², i.e. the sum of the heights of the highest peak and the deepest valley in this area, and inspects the surfaces contacting proppant sand and cenosphere sand respectively. 3D geometry A handheld scanner with a nominal accuracy of ±20 μm was used to acquire point clouds and compare them to CAD models. Retain here is the surface parameters Sz, can't call it directly in along a contour calculation of Rz.
Binder Bridges, Strength, Shrinkage and Casting Quality
Both types of sand are suitable for layering, but their size differs significantly. the average roundness of that proppant sand is 0.74, and that of the float bead sand is 0.78; Small particles and broken spherical shells can be seen in the shape of the latter, and its average wall thickness is about 4 μm. The average particle size was 254 ± 5 μ m and 70 ± 3 μ m respectively. Figure 4 and Figure 5 show the morphology and particle size distribution in combination, indicating that the cenospheres need thinner layups and higher curing agent and binder consumption, not only because the particles are smaller, but also because of the hollow structure.


EDS results are given in atomic percent. the proppant sand is mainly compose of Al and O, and contains Si, Fe, Ti and Ca; Si, Al and O are dominant in cenospheres. These compositional differences were retained in Table 1, and subsequent XRD further confirmed that proppant sand contained corundum and mullite, while cenospheres were characterized by mullite peaks and a distinctly amorphous background. The printed phase is basically the same as the original sand, and the organic resin does not form the same clear crystal peak in XRD because of its high content.
| Sand material | O | Al | Si | Ca | Ti | Fe | Mg | Na | K |
|---|---|---|---|---|---|---|---|---|---|
| Proppant sand | Balance | 26.7 | 3.5 | 0.5 | 0.7 | 1.5 | — | — | — |
| Cenosphere sand | Balance | 12.4 | 17.5 | 0.2 | 0.1 | 0.2 | 0.1 | 0.3 | 0.2 |
Thermogravimetric analysis shows that the total weight loss of proppant sand printing sample is about 1.8%, and that of cenosphere sand sample is about 13%, corresponding to the difference of resin and curing agent mass ratio between the two kinds of samples. The bulk density is about 1.9 g/cm³ and 0.4 g/cm³ respectively. The light weight, hollow and small particle size of cenospheres jointly raise the relative binder demand. The characteristic temperatures of the two types of curves are similar, and the main difference is the weight loss amplitude, rather than the two completely different decomposition mechanisms.
The weight loss of floating bead sample begins at about 100 ℃, which is related to the volatilization of water, residual monomer and oligomer. 300 - 500 ℃ is the maximum weight loss rate range, and the thermal damage of the resin is completed at about 600 ℃. 600 ℃ was chosen as the intermediate heat treatment temperature for scheme Ⅲ. Releasing pores occupied by organic components before infiltration is the fundamental difference between this scheme and increasing the number of infiltrations directly. Figure 6 preserves the correspondence between temperature and mass change.

The results also help to distinguish between "original sand refractory framework" and "bonding bridge formed later". The former comes from corundum and mullite in proppant or mullite and amorphous components in cenospheres, while the latter mainly comes from immersed silica sol. At high temperature, silicon and aluminum oxides may continue to react to form mullite, but there is mullite in the original sand, and the relative diffraction peak has not changed obviously. Therefore, the author does not declare that the newly added reaction amount has been quantitatively confirmed only by the existence of this peak.
XRD after infiltration and sintering shows cristobalite peak. The source of the new peak is related to the colloidal silica added, and the new peak cannot be interpreted as the complete transformation of the original sand. Corundums and mullites remain in proppant sand samples, cristobalite peaks are stronger in cenospheres samples, reflecting that silica sol introduced into the latter has a larger proportion. SEM and EDS also show that the bond bridges between grains are rich in Si and O, which is consistent with the phase determination.

Grain and bridging zone can be seen in fracture of proppant sand scheme Ⅰ and Ⅱ. The microstructure appearance of two and three times infiltration is similar after single view of two-dimensional fracture. The authors point out that it is difficult to quantify binder volume fraction and bridge area from this image alone. Therefore, the similarity of Figure 8 does not mean that the two schemes have the same strength, and it is necessary to continue to combine bending results and internal volume segmentation. The fracture of scheme III shows more bridging and less intergranular voids, which is consistent with the effect of re-infiltration after resin removal.


Micro-CT further revealed heterogeneous infiltration. There are local high porosity areas in proppant sand scheme II sample, which are marked in pink in Figure 12. The author relates this phenomenon to the slow solidification speed of silica sol flowing downward under gravity after taking out the sample. Even if the specimen is wet on the outside, it does not mean that the same amount of binder is retained at each height inside. This observation was later repeated in the case of insufficient strength and cracking of the upper surface of the size profile.

In the reconstruction of 1.2×1.2× 1.2 mm³ representative area of proppant sand, the sand, binder and pore volume fractions are 68.3%, 18.4% and 13.3% respectively. A considerable amount of pores remain between the particles, indicating that the infiltration did not transform the mold into dense ceramics. The porosity of scheme Ⅲ is 21.5%, but the pores are mainly spherical and located in hollow particles. External particles and binder can form a more continuous connection. Therefore, the total porosity of both materials must be understood in conjunction with pore location and connectivity morphology.

For floating spheres, silica sol cannot enter the complete hollow sphere, and the enclosed space in the sphere remains. The outer part of the particles is coated and connected by a binder. This is the structural feature the authors wanted for the riser components: to achieve the required strength while retaining the low density and insulation potential. The measured thermal conductivity of these two types of sintered sand molds is not given in this paper, so this material division should be understood in conjunction with the hollow structure and design purpose, and cannot be written as a certain percentage of the insulation benefit has been quantified.

There is also a practical problem in sand mixing stage: when acid curing agent is added only once before printing, the mechanical properties of printed samples are not ideal. The author suggests adding a part of curing agent first, standing for 24 h, and then adding the second part before printing; It is speculated that the reaction product layer formed by initial contact may reduce the strength of subsequent interaction. The paper regards it as a possible cause, but does not determine the surface reaction as a definite chemical reaction path.
the prin bending strength of that proppant sand is 0.77 MPa, which is enough to complete the operation of taking out and infiltrating. After twice impregnation, the strength was increased to 1.04 MPa, but during re-sintering, the resin burned out and the strength decreased to 0.60 MPa. Scheme Ⅰ could not meet the requirements of shell application. After changing to scheme Ⅱ of three times infiltration, the final sintering strength reaches 3.74 MPa, which is close to the range of about 3 - 6 MPa for the conventional silica sol shell used as reference in this paper. The benefit of multi-infiltration is whether the inorganic bridge after burning can replace the original resin, rather than only improving the wet strength at room temperature.
The as-printed cenosphere sand specimens had a bending strength of 0.56 MPa. Two impregnations raised it to 2.84 MPa, but subsequent sintering reduced it to 1.98 MPa. Regime III added a 600 °C intermediate heat treatment after the first two impregnations, followed by two further impregnations, giving 4.24 MPa after final sintering. Figure 15 compares both materials through the process. The same direct impregnation route was not equally effective for the two sands; the higher organic content of the cenosphere material made the loss of bonding during burnout particularly important.

The strength improvement also brings shrinkage matching problems. The final linear shrinkage of proppant sand scheme Ⅱ is 0.5±0.1%, and that of cenosphere sand scheme Ⅲ is 1.8±0.2%. Both are lower on their own, but the latter is about three to four times higher than the former. The authors link the difference mainly to particle size: finer particles have greater sintering driving force. For a set of sand molds assembled from two materials, the evaluation cannot stop at "the shrinkage is not high," but also whether adjacent parts maintain the same joint size after sintering.
There is also a difference in infiltration scale between small samples and complete molds. Although the immersion time was prolonged to 5 min for the formal model, the longer immersion time did not necessarily prevent the adhesive from continuing to flow downward after removal. The weak area caused by the lack of glue in the upper part needs to be controlled by placing direction, drying and subsequent heat treatment. This paper relates this loss to the high porosity area of CT specimen and the insufficient surface strength of intact part, so the analysis is not only aimed at one accidental crack.
Complete mold fabrication exposes these differences more clearly. After intermediate treatment at 600 ℃, cracks appear and the strength of the upper surface decreases, which corresponds to the lack of binder caused by gravity loss. It is suggested that the orientation of the component should be changed between impregnation and drying to make the adhesive distribution more uniform. aft that proppant sand mold part is finally sintered at the temperature of 1200 DEG C, part of the support corundum sand is agglomerated with the mold surface, so that the cleaning difficulty is increased; Lowering the sintering temperature and using coarser bearing sand are proposed as further improvement directions.

During assembly, the contact between the upper shape of cenospheres and the lower shape of proppant is poor, and there is a gap between the interfaces of components. The impeller castings thus present a thin layer of excess metal, i.e. flash, at the parting line. Figure 17 also shows that the metal has penetrated deep into the mold, and proppant sand particles are visible in the casting. The paper does not equate casting complete impeller with all surface quality reaching the traditional technology level, but lists the problems of block shrinkage, fit and penetration as the conditions to be solved.
To determine the actual shrinkage, this print was not pre-compensated for the casting or mold CAD size. After that, the casting CAD was adjusted by 1.5%, and a smaller deviation was obtained when compared with the scanning point cloud. The deviation in most areas does not exceed 2 mm, and the deviation in the flash of the type exceeds 2 mm. The positive mean deviation +0.57 mm is higher than the negative mean deviation −0.30 mm. The author believes that flash is the main source of deviation asymmetry. This is the result of the geometric registration after the trial, not equivalent to having completed a set of compensation factors verified in production.
Surface measurements also retain limitations. The Sz of contact zone with proppant mold is 152±13 μm, and contact zone with floating bead mold is 115±8 μm. The finer floating bead corresponds to lower roughness, but both of them are higher than the typical level of traditional casting method. Figure 18 shows the coexistence of localized peaks and valleys and flatter regions. Reducing the grain size of the sand and adding coating on the surface of the cavity are the improvement ideas put forward in this paper. These recommendations do not yet represent the further reductions already measured at this time.

The whole experiment establishes a feasible route from organic printing state to inorganic bonding sand mold, and also shows that the material strength, local porosity and integral quality are not simply one-to-one correspondence. The third infiltration of proppant sand and the infiltration of cenosphere sand after middle burning respectively solve the problems of strength after burning. Binder expulsion, support sand adhesion, differential shrinkage and metal penetration still affect the final casting when used in a true multi-material composite mold. Subsequent process design needs to evaluate these links together, rather than selecting only the set of parameters with the highest bending strength.
Viacheslav E. Bazhenov, Ksenia A. Deputatova, Andrey A. Rizhsky et al.; Journal of Manufacturing and Materials Processing,9,96; DOI:10.3390/jmmp9030096。 This article is compiled based on the original text, and the drawings and tables retain their original numbers and are authorized by CC BY 4.0.Original Paper · PDF · CC BY 4.0 ·