Embedding Optical-Fiber Sensors in H13 Die Material: Directed Energy Deposition, Depth Trials and Mechanical Tests


Published: 

2025-02-11

Directed energy deposition embeds AISI-304 tubing in H13 before fiber Bragg grating sensors are inserted. Multipoint temperatures at depths of 1.5–3.0 mm are compared alongside interface, hardness and tensile tests. Measurements extend only from room temperature to 200 °C.

Figure 7 of the original paper: FBG demodulator, control unit and multi-point temperature monitoring system.

Figure 7 of the original paper: FBG demodulator, control unit and multi-point temperature monitoring system.

H13 Specimens, Tube Embedding and Four Sensor Depths

The temperature distribution in the die-casting mold affects filling, cooling and casting performance, but it is difficult to directly describe the entire mold interior with a small number of thermocouples or surface thermal images. The paper hopes to add internal multi-point data and studies a sensor installation method: first bury a thin tube in H13 steel, and then insert the fiber Bragg grating sensor into it. Rather than starting directly with a mass-production die-casting cycle, it first uses a controlled heat bench test to check the temperature response before confirming whether the machined material can maintain the necessary mechanical properties.

Fiber Bragg Grating, or FBG, uses the characteristics of specific wavelength reflection that changes with temperature to convert optical signals into temperature. The diameter of the optical fiber sensor used in the paper is about 250 μm, and the inner diameter of the protective seamless tube is 500 μm. Its small size is conducive to arranging multiple measuring points in a limited space, but the cooperation between the optical fiber itself, the protective tube and the surrounding mold materials will also affect the readings and interface status. Therefore, installation methods and temperature testing must be evaluated together.

The authors cite in the background other studies of FBG being used at higher temperatures, but this trial only heated from room temperature to 200°C. These temperature ranges cannot be combined: the existing high-temperature resistance literature of the sensor does not mean that the buried pipe, deposition and signal acquisition system has been verified in the actual high-temperature die-casting environment. At the end of the paper, high temperature environment and real process applications are still listed as follow-up work.

AISI-H13 is used for both the matrix and the deposited powder. Table 1 of the original text lists the mass fractions: C is 0.5%, Cr is 5.0%, Mn is 0.4%, Mo is 1.6%, Si is 1.0%, V is 1.1%, and Fe is the balance. The powder morphology was observed by SEM. Using the same tool steel for deposition allows comparison of the interface and thermal history around the buried pipe area, rather than adding a completely different surface cladding material.

Original Table 1: Chemical composition of H13 (wt.%)
CCrMnMoSiVFe
0.55.00.41.61.01.1Balance

The DED equipment is InssTek DMT-MX3, including laser and powder feeding units. The paper explains that the equipment uses a 4 kW CO₂ laser, and the actual test process power is set to 850 W according to Table 2. The two are the equipment description and specific working conditions. The rated capacity of the equipment cannot be mistakenly written as the actual power of the test piece. The laser incident diameter is 1 mm, and argon gas with a purity of 99.9% is used for protection and powder feeding.

Original Figure 2: Schematic of directional energy deposition equipment and laser and powder feeding systems.
Figure 2: Schematic diagram of directional energy deposition equipment and laser and powder feeding systems.

Table 2 specifies a powder feed of 5 g/min, a nozzle travel speed of 800 mm/min, a powder carrier-gas flow of 2.5 L/min and a coaxial-gas flow of 8 L/min. Bead height was 0.25 mm and bead spacing 0.5 mm. The same process conditions were used for temperature, hardness and tensile specimens, so the mechanical evaluation corresponds to the deposition route used for tube embedding rather than a separately optimized condition.

Original Table 2: Actual process conditions of DED
ParameterValue
Laser power / W850
Powder feed rate / g·min⁻¹5
Nozzle speed / mm·min⁻¹800
Powder carrier gas / L·min⁻¹2.5
Coaxial gas / L·min⁻¹8

The temperature specimen base is H13 steel of 100×50×10 mm. First, wire cutting is used to process V-shaped grooves and holes of different depths, then AISI-304 seamless pipes are placed, and then DED is used to deposit around and above them. After completion, the surface is processed to make the specimen height consistent, and mirror processing is used to reduce the contact thermal resistance when in contact with the heat source. The fiber is inserted last, rather than exposing the bare fiber directly to the laser deposition stage.

Original Figure 3: H13 slotting, 304 seamless pipe embedding, DED deposition and optical fiber insertion process.
Figure 3: H13 slotting, 304 seamless pipe embedding, DED deposition and optical fiber insertion process.

Figure 4 shows four burial depths of 1.5, 2.0, 2.5, and 3.0 mm from the heated surface. The specimen was placed on the hot stage and raised from about 30°C to 200°C. The temperature changes were then observed for 30 min. Three measuring points were compared for each condition. The study hopes to confirm whether the difference in burial depth significantly changes the response and stable readings, so depth and measuring point are used as two different comparison dimensions.

Original Figure 4: Four buried pipe depths of 1.5, 2.0, 2.5, and 3.0 mm from the heating surface.
Figure 4: Four buried pipe depths of 1.5, 2.0, 2.5, and 3.0 mm from the heating surface.

Also check the cross section after installation. SEM is used to observe the interface near the deposition area, non-deposition area, H13 matrix and seamless tube, and confirm the location of the optical fiber. The paper not only reports on the formation of a bond on the deposited side, but also points out that there are unfilled parts in the undeposited area, and suggests that improvements such as welding can be considered. The absence of pores at a certain observation position cannot be expanded to mean that all areas of the entire piece have reached complete dense connection.

Original Figure 6: Cross-sectional SEM and interface observation of H13 matrix, seamless tube and 250 μm optical fiber.
Figure 6: Cross-sectional SEM and interface observation of H13 matrix, seamless tube and 250 μm optical fiber.

In conjunction with the temperature test, the hardness test pieces adopt deposition heights of 1, 2, and 3 mm. Each layer is 0.25 mm, so it corresponds to layers 4, 8, and 12 respectively. This height grouping is used to examine the effects of deposition times and thermal exposure on materials, and is not the same set of geometric quantities as the 1.5–3.0 mm sensor burial depth in the temperature test. If the two are combined directly, it is impossible to accurately trace which test piece a certain hardness result comes from.

Original Figure 5: Preparation of 1, 2, and 3 mm hardness specimens and tensile specimens with deposition zone.
Figure 5 Preparation of 1, 2, and 3 mm hardness specimens and tensile specimens with deposition zone.

Tensile specimens were prepared in accordance with ASTM E8 and deposited in grooved specimens according to the method cited in the original text and then processed into the test shape. There are five pieces each in the deposited group and the undeposited H13 group. The authors used fracture locations and stress-strain curves to check whether the deposition-related areas became obvious weak points, not just to confirm that the sensor could read the temperature.

Multipoint Response, Hardness and Tensile Results

The temperature measurement system includes FBG demodulator, control unit and temperature measurement software. The paper describes that the demodulator has 12 channels and can collect up to 600 optical signal data in real time and convert it into temperature display through the program. This expression refers to the channel and data capabilities of the acquisition system, not the 600 sensors that have been embedded in the mold this time, nor the 600 Hz sampling frequency given in the paper.

Cross-section Figure 6 shows a 250 μm optical fiber inside a seamless tube. The deposition is based on the interface near the central axis of the tube, forming a bond above; no obvious pores are found in the observed deposition interface. Since there are still unfilled positions on the non-deposition side, this set of observations supports the feasibility of the mounting route on the one hand, and also shows that the complete packaging details can continue to be improved. The paper does not give a unified defect volume fraction after three-dimensional non-destructive inspection of the entire mold.

It takes about 800 s for the sensor 1.5 mm away from the heat source to reach temperature stability, and there is no obvious temperature difference between the three measuring points. The three groups of 2.0, 2.5, and 3.0 mm also experienced a stable process of about 800 s, and finally each point reached the set temperature, showing no obvious difference in burial depth sensitivity. Figure 8 retains four sets of curves over time, rather than just comparing the last temperature value.

Original Figure 8: Temperature-time curves of three measuring points at four burial depths.
Figure 8: Temperature-time curves of three measuring points at four burial depths.

Based on this, the author believes that the appropriate layout position can be selected within the test range of 1.5–3.0 mm, and multi-point temperatures can be collected in real time, and the signal loss does not have a significant impact on the results. However, about 800 s is the stabilization time formed by the heating of the hot stage, the heat transfer of the specimen and the sensor readings. It should not be directly called the inherent response time of the optical fiber sensor itself, let alone claim to have captured every transient thermal peak of high-speed die casting.

The temperature results also have clear conditions: the heat source is a hot stage, the surface of the specimen is processed to a maximum of 200°C, and the observation time is 30 minutes. Repeated thermal cycles, mechanical loads and higher temperatures found in actual die casting were not all reproduced in this set of tests. Therefore, the paper gives the experimental basis for internal multi-point layout and data acquisition. In the future, the system needs to be put into real working conditions to verify the long-term stability.

The hardness is measured using the Rockwell method in the deposited area and undeposited matrix area. The deposited area in Figure 9 is significantly higher than the undeposited area, reaching and exceeding the 50 HRC used by the author as a reference for mold suitability. The article relates this change to the thermal effect of the deposition process, and reviews existing research on H13 at approximately 55 HRC under relevant heat treatment conditions, but does not regard the heat treatment results of other studies as accurate readings for each measurement point this time.

Original Figure 9: Rockwell hardness of the deposition area and matrix area at various deposition heights.
Figure 9: Rockwell hardness of the deposition area and matrix area at various deposition heights.

1T, 2T, and 3T represent deposition heights of 1, 2, and 3 mm, among which 3T has a higher substrate hardness. The author believes that more layers means longer processing time and heat exposure, and the impact does not only occur on the additional metal layers. Higher hardness can support usage requirements, but excessive hardening may introduce brittleness, so the paper also proposes that the hardness needs to be controlled within an appropriate range through alloy composition and process parameters, rather than simply pursuing the highest value.

Table 3 of the original article lists the tensile results piece by piece. The tensile strengths of the five undeposited pieces are 648.495, 640.947, 644.851, 663.211, and 641.034 MPa; the tensile strengths of the deposited group are 656.134, 664.436, 647.983, 666.349, and 647.804 MPa. The numerical ranges of the two groups overlap. Therefore, when understanding the author's conclusion, the fracture position must also be considered, and you cannot just select the highest value of each group for comparison.

Original Table 3: Piece-by-piece stretching results
SpecimenTensile strength / MPaStrain (original heading)
Not deposited H13-1648.4950.4616
Not deposited H13-2640.9470.5104
Not deposited H13-3644.8510.51
Not deposited H13-4663.2110.4952
Not deposited H13-5641.0340.4764
Deposition H13-1656.1340.4676
Deposition H13-2664.4360.4404
Deposition H13-3647.9830.4488
Deposition H13-4666.3490.4396
Deposition H13-5647.8040.4492

Figure 10 shows that the two groups of stress-strain curves have similar shapes, and the fracture of the deposited sample occurs in the undeposited area. The five deposited specimens all showed the same trend, which led the authors to believe that the tensile load-bearing capacity of the deposited area was higher than that of the undeposited part that fractured first. This judgment comes from the failure position of the entire specimen, and does not mean that the interface material has been taken out separately and its independent tensile limit has been measured.

Original Figure 10: Tensile fracture positions, stress-strain curves and comparisons of the two groups.
Figure 10: Tensile fracture positions, stress-strain curves and comparisons of the two groups.

The other column in Table 3 is labelled Strain. Its original values, including 0.4396–0.5104, and heading are retained. The table does not define all conversion conventions, so these values are not relabelled as percentage elongation after fracture. This preserves the distinction between a strain value on a curve and a separately defined material acceptance measure.

Taken together, the buried pipe plus DED method integrates the sensor channel into the H13 specimen and obtains similar stable multi-point readings at the measured burial depth. Interface observation and hardness and tensile comparisons show that the deposition area did not become the weakest location for the first failure of this specimen. Temperature and mechanical evidence complement each other and are closer to the information needed to evaluate mold interior mounting options than a temperature curve alone.

The next step in the research is to use the temperature measurement system in actual die casting and continue to study other process parameters and hardness control. The current results support the potential application of this installation and monitoring route, but its scope of application is still jointly defined by hot stage temperature, specimen geometry, deposition conditions, and test quantity. For specific molds, subsequent verification should check the signal, interface and material changes in the real temperature cycle, rather than just using the conclusion from room temperature to 200°C.

Jihoon Jang, Gyeong-Yun Baek; Journal of Materials Engineering and Performance, 34, 8988–8995; DOI: 10.1007/s11665-025-10772-y. This article is compiled based on the original text. Figures and tables retain their original numbers and are licensed under CC BY 4.0.Original paper · PDF direct · CC BY 4.0 ·