Gases from Printed-Pattern Burnout: VOCs and Thermal Decomposition of Six Polymers


Published: 

2024-10-09

Field passive sampling and TG–FTIR compare HIPS, ABS, PLA, PP, PA12 and wax-containing PMMA. Additives and background influence profiles; burnability or low residue alone cannot establish emissions.

Figure 1 . Printed patterns, burnout furnace and field samplers.

Figure 1 . Printed patterns, burnout furnace and field samplers.

Patterns, Production Burnout and Two Gas-Analysis Routes

Printed investment-casting patterns introduce thermoplastics/additives beyond traditional wax. This study compares commercial HIPS, ABS, PLA, PP, PA12 and powder-printed PMMA. Field organic sampling is combined with controlled thermal-decomposition analysis, connecting actual process exposure with material stability rather than judging low emissions from a product name.

HIPS/ABS/PLA/PP/PA use Zortrax ZM200 FDM with 1.75 mm filament and 0.4 mm nozzle. Voxeljet VX500 uses mean 50 μm PMMA/PEMA-blend powder, then hydrocarbon/paraffin wax infiltration, melting near 55 °C. Thus it is not pure PMMA versus five ideal pure polymers; fillers, rubber modifiers and wax can affect products.

Patterns are embedded in gypsum in steel cups, vacuum-degassed 5 min and cured, then burned out in a Nabertherm 150 WAX at 720 °C for 4 h. Industrial extraction ventilates the hall for 8 h, with subsequent runs on 24 h cycles. Figure 1 shows patterns, furnace and samplers. Results concern this site, ventilation and program, not a universal foundry emission amount.

Three radiello passive diffusion samplers operate for 6 h without power/gas, limiting disturbance. Carbograph 4 is 300±10 mg, 35–50 mesh. Sealed tubes go to laboratory two-stage thermal-desorption GC–MS. This collects species over an interval rather than second-by-second furnace concentrations.

Desorption uses 290 °C/15 min into a 0 °C microtrap with helium 50 mL/min, then 300 °C/5 min, splitless helium 1.0 mL/min into Agilent 6890 GC. Column dimensions are 30 m×0.25 mm×1 μm. Oven: 50 °C/1 min, 10 °C/min to 120 °C/2 min, then 15 °C/min to 280 °C/5 min. MS uses SCAN; only NIST spectral matches above 85% support qualitative interpretation.

TG–FTIR heats about 10 mg in air 30 mL/min from 30 to 900 °C at 10 °C/min. STA connects to TENSOR 27 through a 230 °C line and 200 °C cell to limit condensation. TG tracks mass, DTG mass-loss rate and IR functional groups. This differs from 720 °C field burnout/6 h sampling; decomposition temperature is not the time of peak workplace concentration.

Background is established by heating gypsum without a printed pattern, then subtracted from material chromatograms. Building products, other polymers and surface-adsorbed residues can emit organics. Distant toluene/benzaldehyde signals might otherwise be assigned wrongly to the current pattern. Figure 2/Table 1 describe background, not emissions entirely from new patterns.

Figure 2 . Background chromatogram from blank gypsum burnout.
Figure 2 . Background chromatogram from blank gypsum burnout.

Material Profiles, Mass Loss and Process Selection

Background-subtracted HIPS retains many low-mass species. Styrene dominates, with benzene, toluene, ethylbenzene, α-methylstyrene, xylenes and naphthalene. Aromatics relate to chain scission, dimerization/trimerization and cyclization; benzaldehyde/phenol/acetophenone relate to oxidation. Polybutadiene modification can also yield aliphatics, so one monomer cannot explain a commercial modified grade.

Figure 3 . Background-subtracted HIPS chromatogram.
Figure 3 . Background-subtracted HIPS chromatogram.

ABS resembles HIPS because both contain styrenic/butadiene structures, but benzonitrile appears near retention time 8.4 min and some later hydrocarbons are weaker. These are structural/compositional differences. GC retention time is laboratory separation time, not onset of gas release 8.4 min after burnout; field exposure lasts 6 h.

Figure 4 . Background-subtracted ABS chromatogram.
Figure 4 . Background-subtracted ABS chromatogram.

PLA resembles background, with fewer derivative signals including acetic acid and carboxylic esters. Toluene, benzaldehyde and decane are prominent distantly at c but scarce near the furnace, favoring background origin. PP also resembles background, with little detected at c about 7 m away; enhanced signals include decane, undecane, dodecane and longer aliphatics. Lower detection does not mean every gaseous product is zero.

Figure 5 . Background-subtracted PLA chromatogram.
Figure 5 . Background-subtracted PLA chromatogram.
Figure 6 . Background-subtracted PP chromatogram.
Figure 6 . Background-subtracted PP chromatogram.

PA field signals are low, potentially involving crosslinking, conjugation and nonvolatile char. Absence of certain nitrogen compounds by this method does not exclude small nitrogenous gases. Wax-containing PMMA mainly gives methyl methacrylate plus aromatics and longer hydrocarbons, the latter influenced by paraffin. Infiltration is therefore part of the comparison boundary.

Figure 7 . Background-subtracted PA chromatogram.
Figure 7 . Background-subtracted PA chromatogram.
Figure 8 . Background-subtracted wax-PMMA chromatogram.
Figure 8 . Background-subtracted wax-PMMA chromatogram.

Table 2 reports 5/10/50% mass-loss temperatures, DTG peaks/rates and 900 °C residue. HIPS gives 339/359/411 °C, 417 °C at 17.47%/min and 534 °C at 0.63%/min, residue 4.4%. ABS gives 371/390/422 °C, table peak 423 °C at 19.93%/min and 561 °C at 1.37%/min, residue 0.6%. Peak and fractional-loss temperatures are different metrics, not one “decomposition temperature.”

Table 2. TG/DTG results and residue at 900 °C
MaterialT5% / ℃T10% / ℃T50% / ℃DTG1 / ℃;%/minDTG2 / ℃;%/minR900 / %
HIPS339359411417;17.47534;0.634.4
ABS371390422423;19.93561;1.370.6
PLA_grey330340371375;70.70—0.1
PP299322384401;15.80691;1.099.7
PA397417460464;15.34—0.1
PMMA + paraffin231247336275;7.92389;11.200.1

PLA_grey has 330/340/371 °C fractional-loss temperatures, table peak 375 °C at 70.70%/min and residue 0.1%. PA has 397/417/460 °C, 464 °C at 15.34%/min and 0.1%. PA’s highest T5% means later significant loss under these conditions. Low field PLA emissions and high PA thermal stability are separate dimensions, not universal superiority.

Figure 9 . TG mass-loss curves of six materials.
Figure 9 . TG mass-loss curves of six materials.
Figure 10 . DTG mass-loss-rate curves of six materials.
Figure 10 . DTG mass-loss-rate curves of six materials.

PP gives 299/322/384 °C, peaks 401 °C at 15.80%/min and 691 °C at 1.09%/min, residue 9.7%, the highest. The later stage is associated with calcium-carbonate filler. Wax-PMMA gives 231/247/336 °C, peaks 275 °C at 7.92%/min and 389 °C at 11.20%/min, residue 0.1%. Earlier wax-related and later PMMA stages show additives affect onset, shape and residue.

All materials show IR bands of CO₂, H₂O and CO, so low organic chromatographic signals do not mean those gases are absent. CO₂ appears around 2400–2300 and 670 cm⁻¹, water 4000–3500/2000–1500, CO 2200–2100. PLA has ester/methyl/carbonyl bands at 1183/1457/1750 cm⁻¹. Weak PA features near 950 and 1460–1600 may indicate ammonia but overlap water, preventing unambiguous single-species quantification.

Figure 11 . Temperature-resolved FTIR and spectra at major peaks.
Figure 11 . Temperature-resolved FTIR and spectra at major peaks.

This is species screening/thermal comparison, not a complete exposure-dose assessment or exhaust-system design. NFPA/GHS, vapor pressure and flash point describe hazards of detected substances, distinct from actual inhaled dose at a factory. Material, additives, burnout, background and collection/treatment conditions require joint evaluation.

The paper suggests targeted collection/filtering/adsorption for ABS/HIPS/PMMA, recognizing treatment selectivity, or lower-field-signal PLA/PA when performance permits. This does not remove ventilation/control requirements: TG–FTIR still finds gases. Low residue, lower organic signals, printability and shell quality are parallel criteria, not substitutes.

Adsorbent tubes are sealed in glass immediately after sampling to limit loss. TD transfer is 160 °C, GC–MS line 280 °C, ion source 230 °C and quadrupole 150 °C. The full transfer/separation chain affects comparability. Library-match threshold is qualitative identification, not detection percentage or concentration.

Background contains aromatics, aliphatics, terpenes and oxygenates. Flooring/building materials, rubber, foam, polystyrene/polyester and wood can contribute. A compound can originate from current decomposition or prior room sources, hence blank-gypsum heating rather than raw spectra as a material fingerprint. Spatial comparisons also require the same sampling procedure.

Definitions of VOC vary by boiling point/vapor pressure; some longer, higher-mass hydrocarbons do not qualify under every definition. They remain detected organics. Vapor pressure describes evaporation tendency; flash point concerns formation of ignitable vapor under standardized conditions. Neither is proof of an attained hazardous workplace concentration.

First-stage HIPS IR bands relate to toluene/ethylbenzene/styrene; most disappear later, mainly leaving CO₂/CO. ABS aromatic/aliphatic bands also weaken in its second stage. This connects field polymer signatures with controlled thermal timing, but different instruments/sampling principles prevent direct conversion of an IR band into a field organic concentration.

Wax-PMMA shows early C–H/C=O/CH₂ bands at 2931/1741/1470 cm⁻¹ and small 310–340 °C DTG features associated with paraffin. Infiltration adds decomposable material before burnout. Pure-resin handbook temperatures alone miss this and cannot explain the two observed stages.

Burnout-pattern selection therefore needs grade-specific decomposition knowledge alongside accuracy/finish. The evidence shows different profiles and the importance of background/additives. Bio-based PA is a future comparison, not an already tested result. Production should preserve material/test boundaries and validate actual burnout/exhaust conditions.

Source: . Analysis of emission of volatile organic compounds and thermal degradation in investment casting using fused deposition modeling (FDM) and three-dimensional printing (3DP) made of various thermoplastic polymers. 2024-10-09. DOI: 10.1007/s11356-024-35200-x. Adapted from the open-access paper; original figure/table numbers retained. CC BY 4.0.Original paper · Direct PDF · CC BY 4.0 ·