3D Sand-Printed Risers: Feeding Performance of Spherical Designs
Published:
2024-05-15
Compare five types of risers for nickel aluminum bronze, carbon steel and aluminum alloy, and analyze the feeding capacity and process yield based on tube shrinkage, critical solid phase rate time and Niyama criterion.
Figure 3 . CAD dimensions of cylindrical, ellipsoid, spherical, compound and inverted conical risers.
Three-dimensional riser design and solidification evaluation method
Three-dimensional sand printing can create riser shapes that are difficult to achieve with traditional mold drawing methods, so that riser design does not have to be limited to cylinders that are easy to draft. The study compared five types of risers: cylindrical, ellipsoidal, spherical, composite and inverted cone, and analyzed the effects of different shapes, riser neck dimensions and superheat on feeding through solidification simulation. The materials are C95800 nickel aluminum bronze NAB, A216 WCB carbon steel and A319 aluminum alloy. The three represent different solidification intervals, so the optimal shape of one material cannot be used to infer the feeding performance on all alloys.
The study first divided the shrinkage problem into two aspects: main insulation and channel maintenance. Due to the different sizes and shapes of castings, the final solidified liquid metal may be isolated from the surrounding areas and risers; after the dendrite network is formed, the liquid supply is blocked, eventually leaving isolated shrinkage cavities. The riser is not part of the final part. Although increasing the volume of the riser may increase the feeding allowance, it will also reduce the process yield. There is a direct design trade-off between the need for the riser neck to remain connected when the casting needs to be fed, but also the desire to have a smaller cross-section that facilitates subsequent removal. The comparison of three-dimensional shapes revolves around this contradiction.
The paper reviews the traditional methods of improving solidification by adjusting cylinder size, setting up chill or insulation measures, as well as topology optimization, CAD/CAE joint design and other routes. Some of the existing methods iteratively optimize from an initial riser that is too large, some first predict the isolated liquid phase region and then generate the riser geometry, and some research also incorporates the casting structure, alloy, chill and core into the design. The theoretical insulation advantages of hemispherical and spherical shapes have been studied, but their internal shrinkage may reduce the actual feeding effect of the top riser. Therefore, in addition to comparing the solidification time, this article also directly compares the shrinkage pipe position and the pore results after feeding to avoid equating the thermal advantages of the ideal geometry with the final casting quality.
The analysis of solidification time is based on the Chvorinov relationship. The original formula (1) relates time to the square of the volume/surface area ratio. The proportional term includes the latent heat of solidification, the thermal physical properties of the metal and the sand mold, and the difference between the melting point of the metal and the initial temperature of the sand mold. After considering the pouring superheat, the original equation (2) further incorporates the specific heat of liquid metal and the sensible heat corresponding to the additional superheat. For different geometries of the same volume, smaller surface area means higher modulus, but local temperature gradients, neck size, and shrinkage development can also change the effective feeding process. The study therefore set up additional superheat conditions of WCB to check whether the overall solidification time and CFST change in the same way.
The selection of the initial dimensions of the riser neck is also based on the literature. The recommended modulus range reviewed in the paper is 1.1-1.5 times the casting modulus; the riser neck modulus of ductile iron may be as low as 67% of the casting modulus and cannot be mixed with other alloys. Under the assumption of a relatively high safety margin and a modulus of approximately 1.5 times the casting, the riser neck diameter of the steel casting can be approximately 60% of the main body diameter; the article also points out that industrial design is often based on 1.2 times the casting modulus. The goal of this paper is to find smaller necks that can still be successfully fed without destroying the temperature gradient and sequential solidification. The final judgment depends on the simulation results of each material, rather than treating these empirical ratios as invariant constants.
The study divided the solidification interval into a short interval less than 50°C, a medium interval between 50-110°C, and a long interval greater than 110°C. NAB belongs to the short solidification interval, WCB is the medium interval, and A319 is the long interval. The material in the short solidification interval is more likely to form a shell and advance from the outside inward. The mushy zone of the material in the long solidification interval is wider and may cross the riser or the casting section; the medium interval has the characteristics of both. The simulation uses SOLIDCast 8.9.0 and its default material properties, and uses the finite difference method to calculate cooling, feeding, and shrinkage cavity formation. All solutions are closed mold conditions, and the sand mold thickness is uniformly 2 inches.
The evaluation uses the material density function MDF, critical solid phase rate time CFST and Niyama criterion at the same time. MDF calculates macroscopic pores based on local liquid shrinkage and feeding flow: 0 means completely void, 1 means completely metal. CFST focuses on when the inter-dendritic feeding channels fail, rather than waiting until all solidification to determine the liquid supply capacity. The typical critical solid phase rate of ordinary carbon steel is about 50%, that of aluminum alloy is about 20%-30%, and that of copper alloy is about 25%-35%. The time ST to reach the solidus line is different from the time CFST to reach the critical state of feeding. The latter is more directly related to whether the riser can still deliver liquid metal to the mushy zone.
The Niyama criterion retains the relationship of the original formula (3): Ny = G/√(dT/dt), where G is the temperature gradient in ℃/cm, dT/dt is the cooling rate in ℃/s, and the unit of Ny is (℃·s)¹ᐟ²/cm. When the value is lower than the corresponding critical range, the risk of shrinkage cavities or shrinkage porosity is higher. The critical range used in this paper is 0-1 for steel, 0-0.30 for aluminum alloy, and 0-1.30 for copper alloy. This criterion does not directly consider gravity and may produce uncertain results for low-density materials. Therefore, the author does not rely on one criterion to evaluate all alloys, but compares it with MDF and CFST. The interface heat transfer calculation uses the original formula (4): Q=UA(T₂−T₁), U is the heat transfer coefficient, A is the heat transfer area, and the temperatures of adjacent calculation units are T₁ and T₂ respectively.
Figure 3 retains the riser geometry and size definitions. The experimental design includes two types of cylindrical risers, three types of ellipsoidal risers, four types of spherical risers, as well as one composite and one inverted conical riser. All risers are located in the center of the 6-inch x 6-inch x 1.5-inch flat plate and are fed in all directions as top risers, with a uniform riser neck height of 0.75 inches. The two horizontal semi-axes of the ellipsoid riser are equal, and the geometric effect is studied by changing the ratio of the vertical semi-axis and the horizontal semi-axis. Spherical SR1, SR2, and SR3 focus on comparing riser necks, while SR4 and cylindrical CR2 are used to compare high yield solutions after reducing riser volume.
Except for the special weight reduction plan, the volume of each riser is kept consistent to separate the effects of shape and metal dosage. Table 3 lists the volume, surface area, modulus and modulus increase. The modulus is defined as V/A. The calculation only includes the riser body and does not include the riser neck. The benchmark cylinder CR has a volume of 68 in³, a surface area of 92.23 in², and a modulus of 0.74 in; the main body volumes of SR1-SR3 are both 68 in³, and the modulus is about 0.84 in, which is an increase of 14.47% relative to the benchmark. The modulus from ER1 to ER3 decreases in sequence. Both the SR4 and CR2 have a volume of 47 in³, so the feeding performance of spherical and cylindrical shapes can be compared at the same reduction level.
Under the same volume, cylindrical risers usually provide greater vertical height and are easier to set positive draft angles; spherical bodies have smaller surface areas and higher modulus. The composite riser attempts to take into account the thermal insulation advantages of the spherical shape and the height of the cylinder. The boundary conditions of a closed riser are different from those of a riser where the top surface is in direct contact with the atmosphere, and the dimensions cannot be applied indiscriminately. This study uses unified castings and boundary conditions to compare these factors. The focus is to test whether the geometric freedom released by 3D printing can improve feeding, rather than simply judging the design to be effective based on "small surface area of the sphere."
Feeding results, riser neck and superheat
Figure 4 shows the isothermal distribution of each material and each scheme. In NAB and WCB, the edges and corners of the top surfaces of cylinders and composite risers solidify earlier; A319 shows a different pattern of solidification starting from the center of the top surface. Spheres and ellipsoids do not have the same sharp corners, so local solidification caused by these corners does not occur. The NAB and WCB plates formed a solidification zone earlier, and A319 advanced from the edge away from the riser toward the riser. SR1 has the smallest riser neck cross-section and solidifies faster among all materials. This shows that the thermal insulation capacity not only depends on the shape of the body, but also the neck connecting the castings can become a weak link in the feeding channel.

Figure 5 shows the shrinkage pipe shape and safety margin based on MDF. NAB and WCB form a sharper cone-shaped shrinkage pipe, while A319's shrinkage pipe is blunter and closer to a ball shape. In the figure, the distance from the bottom of the riser neck to the lowest point of the shrinkage pipe represents the safety margin. The allowed shrinkage pipe in the riser should not be directly equated to the scrapping of the casting. NAB has a narrow solidification interval, a sharp shrinkage pipe, and a small safety margin; A319 has a larger margin under the same geometry. SR2 increases the safety margin of the shrinkage pipe design of NAB, WCB and A319 by 11%, 8% and 18% respectively, and no corresponding pores appear in the riser neck. In SR3, the relevant shrinkage pipe height of NAB is 47% higher than that of A319, which again reflects the material difference.

Compared with the cylindrical standard, the shrinkage safety of the inverted tapered riser is improved by 25%, 11%, and 11% for the three materials, respectively, but the overall yield rate is not better than the spherical solution. The reduced spherical SR4 performed successfully for all three alloys in the MDF results in Figure 5, and the paper reported it as a solution to increase the yield by 45%; the cylindrical CR2 of the same volume failed in WCB due to macro pores. The composite shape can achieve shrinkage on all three materials, but the overall performance is close to the benchmark cylinder without equally outstanding improvements. Therefore, whether there is still a continuous feeding channel after reducing the amount of metal needs to be evaluated together with the main body shape.
The CFST results in Figures 6 and 7 reveal the difference in the process of incomplete expression of MDF. In SR1, due to premature solidification of the riser neck in NAB and WCB, the connection between the riser and the casting is lost. NAB has lower thermal conductivity and thermal diffusivity and slower cooling, so the corresponding CFST is higher. For A319, liquid metal remained in the riser after complete solidification of the slab; one reason is that the study used similar riser volumes to facilitate comparison across materials, and these dimensions are higher than typically recommended for aluminum alloys. Therefore, the larger remaining liquid in the aluminum alloy riser cannot be directly explained as its geometric design is better for all working conditions.


Under similar riser neck sizes, the CFST of SR2 is increased by 6%, 4%, and 10% respectively compared with the baseline CR for NAB, WCB, and A319. Some ellipsoid solutions have also been improved. NAB's ER2, WCB's ER3 and A319's ER1 performed better, but the overall advantages of ellipsoids are not as clear as spherical ones. Although the CFST of SR3 is better, it uses a larger riser neck, which needs to be taken into account the difficulty of removal; the improvement in composite shape is less than 1%. It is worth noting that although SR4 was successful in the MDF results, mushy areas still formed in the necks of NAB and WCB, and there was a risk of shrinkage extending to the riser neck or even the casting. Different evaluation results need to be interpreted together, and one picture that is beneficial to the design cannot be retained.
The Niyama results in Figure 8 predict a higher macroscopic pore risk for A319, which is not completely consistent with MDF and CFST. The author believes that this supports the view that there may be uncertainty when this function is used for low-density alloys, and further reference should be made to MDF for aluminum alloys. The Niyama value of the NAB center is close to 1.3, and combined with MDF, its macroscopic shrinkage risk is low. Except for SR1, most WCB solutions have almost no shrinkage cavities inside the flat plate; the predicted shrinkage cavity area of SR2 is 12.67% lower than that of the benchmark cylinder. However, the predicted shrinkage area of SR2 in NAB is higher than the benchmark, indicating that the best result on one material cannot directly replace the independent judgment of another material.

Figure 9 further compares riser necks. A319 can achieve feeding when the ratio of neck diameter to main body diameter is 0.25, and the literature recommended value is 0.40; the same ratio of 0.25 fails in NAB and WCB, and the lowest ratio of success in this simulation is 0.34. Compared with the recommended size cited in the paper, the diameter of the spherical riser neck is reduced by 32%, 77%, and 60% for NAB, WCB, and aluminum alloys respectively, which is beneficial to removing the riser. However, if the neck is too small, it will freeze in advance. Therefore, the distance between the riser and the casting and the heat shielding conditions need to be adjusted. We cannot simply pursue cutting convenience and ignore the interruption of liquid supply.

WCB's SR2 scheme was also used to study superheat, with other design parameters remaining unchanged. Table 5 retains the complete calculation results: superheat degrees of 0, 25, 50, and 75°C correspond to initial temperatures of 1539, 1564, 1589, and 1614°C, CFST are 9.0, 9.7, 10.2, and 10.8 min respectively, and ST is 16.6, 18.4, 19.4, and 20.4 min respectively. In the results section of the paper, the ST change is summarized as about 6% or about 1 minute for every 25°C increase in superheat, and the CFST change is summarized as about 5%-7%; the percentages in the table are listed based on zero superheat. When using, the increase in adjacent operating conditions and the cumulative increase in base operating conditions should be distinguished.
This study is a comparison of solidification simulations, and the authors list physical test verification as work in progress. Its value lies in simultaneously displaying the relationship between the main body modulus, shrinkage pipe position, neck connectivity, material solidification interval and yield rate, and pointing out that different criteria may produce inconsistent results. Three-dimensional printing can provide more free riser geometry, but production applications still need to design and verify the local thermal joints, wall thickness, alloy and batch size of the casting. The shrinkage ratio or yield improvement in a certain flat plate simulation cannot be directly regarded as a universal guarantee for all castings.
variable | Riser scheme and abbreviation | Volume, V (in3) | Surface Area, A (in2) | Modulus M, (in) [V/A] | Modulus increase (%) | |
|---|---|---|---|---|---|---|
Casting | 54.00 | 108 | 0.50 | - | ||
riser shape | Cylindrical riser (CR) | 68.00 | 92.23 | 0.74 | 0 (baseline) | |
Ellipsoid riser 1 (ER1) | 68.00 | 80.84 | 0.84 | 14.09 | ||
Ellipsoid riser 2 (ER2) | 68.00 | 82.19 | 0.83 | 12.22 | ||
Ellipsoid riser 3 (ER3) | 68.00 | 84.59 | 0.80 | 9.03 | ||
riser neck | Spherical risers 1, 2, 3 (SR1, SR2, SR3) | 68.00 | 80.57 | 0.84 | 14.47 | |
Composite riser (FR) | 68.00 | 90.19 | 0.75 | 2.26 | ||
Inverted cone riser (IT) | 68.00 | 85.92 | 0.79 | 7.34 | ||
Volume | Spherical riser 4 (SR4) | 47.00 | 62.98 | 0.75 | 1.22 | |
Cylindrical riser 2 (CR2) | 47.00 | 72.10 | 0.65 | −11.6 | ||
Superheat (°C) | Initial temperature (℃) | CFST(min) | CFST growth rate (%) | ST(min) | ST growth (%) |
|---|---|---|---|---|---|
0 | 1539 | 9.0 | – | 16.6 | – |
25 | 1564 | 9.7 | 8 | 18.4 | 11 |
50 | 1589 | 10.2 | 13 | 19.4 | 17 |
75 | 1614 | 10.8 | 20 | 20.4 | 23 |
Source: Shuvo, Md Moinuddin, King, Philip, Voigt, Robert, Manogharan, Guha. Toward Reducing Casting Defects via 3D Risers via 3D Sand-Printing: A Simulation Study. 2024-05-15. DOI: 10.1007/s40962-024-01353-1. Adapted from the open-access paper; original figure/table numbers retained. CC BY 4.0.Original paper · PDF · CC BY 4.0 ·
Related News