Linking Austenite Grains, Graphite and Dendrites in Gray Iron Castings


Published: 

2024-04-22

The spherical steel shell specimen was combined with direct isothermal quenching after solidification, two-dimensional FFT and EBSD to investigate the relationship between the columnar zone, equiaxed zone and fine graphite band.

Figure 1 . Spherical steel plate mold.

Figure 1 . Spherical steel plate mold.

Melting, tissue retention and image quantification

LGI melt is prepared in an induction furnace with a capacity of 80 kg from raw materials such as high-purity pig iron, FeSi, FeMn, FeS, Cu, and steel sheets. The resulting chemical compositions are listed in Table 1. The materials are prepared in three batches, indicated by the letters A, B and C in their names. In batch C, the initial carbon content of the melt was gradually diluted by adding steel sheets and alloying to form C1-C3. When the melt is ready (between 1400 and 1448 °C), approximately 10 kg is poured into the preheated ladle and transferred to the experimental setup. In batch B, 60 g of a commercially available inoculant (ferrosilicon containing 0.6-1.0 wt% Sr) was added to the bottom of the ladle before pouring the melt. The experimental setup has been described elsewhere. Essentially, it is an instrument designed to measure temperature and volume changes in spherical castings, although volume change measurements are not analyzed in this article. The spherical steel plate mold (Fig. 1) is immersed in the LGI melt, which enters through the hole in the top. The sealed steel tube is connected to an inner cover that is larger than the hole in the mold. After filling the mold, raise the tube, close the lid from the inside and place the sphere in the desired position. An N-type thermocouple inside the tube measures the temperature at the center of the sphere with an accuracy within ±2.2 K according to the manufacturer. An infrared (IR) pyrometer measures temperature at three evenly spaced locations along the equator. The infrared pyrometer was calibrated on an empty steel mold heated to 500–1200 °C in a laboratory furnace and demonstrated accuracy within ±3 K.

When the surface measured temperature dropped to between 847 and 966 °C, the spheres were removed from the instrument and subjected to direct post-solidification austempering (DAAS). The slightly modified DAAS process is 1: rapid transfer of the separated spheres to a laboratory furnace and isothermal holding at 920 °C for 30 min to balance the temperature gradient; 2: water quenching for 14 seconds; 3: rapid transfer to a liquid salt furnace, immersed in liquid salt and isothermal holding at 360 °C; 4: final air cooling to room temperature. Water quenching (step 2) is not a standard procedure for DAAS but was found necessary to avoid the growth of ferrite/pearlite when immersed in liquid salt. This may be related to the very fine graphite in the casting, which acts as a carbon sink and therefore requires faster quenching to suppress ferrite and pearlite. It should be emphasized that water quenching for too long can lead to the formation of martensite. Panoramas of each cross section were captured using a Schottky field emission gun electron microscope (Tescan LYRA3) programmed to capture an array of backscattered electron images with 10% overlap. The magnification and resolution used provided images of 1024 × 1024 pixels with a pixel length of 0.977 µm. The center of the raw captured image is slightly brighter, which is problematic for microscopic tissue quantification. To address this issue, flat-field correction was applied to each image. The basis of the correction is a Gaussian blur of the non-edge image mean, representing the brightness deviation on the image. The corrected images were stitched into a panorama using Image Composite Editor 2.0.3.0.

A method was developed to obtain a macroscopic profile of how graphite size changes across a cross-section. The process is shown in Figure 2. A discrete 2D fast Fourier transform (2D-FFT) is applied to decompose the image (Fig. 2a) into discrete wave sums. A new image (transformed image) is then synthesized, in which the intensity of each pixel represents the logarithm of the amplitude of the wave (related to the absolute peak amplitude), and the proximity to the center of the image is related to the wavelength (Figure 2 b). In such images, the 2D-FFT of finer microstructure images tends to be brighter near their boundaries. Measurements of boundary brightness (and hence the content of fine microstructure) can be calculated as the average of the transformed image weighted towards its boundary. A weight matrix was constructed, as shown in Figure 2c, where the weights rise from zero (black) at the center to one (white) at the edge of the weight matrix, proportional to the distance from the center. Weights away from the center are set to zero (black) to avoid anisotropy associated with the image diagonals. The transformed image is then multiplied element-wise by the weight matrix (Fig. 2d) and then averaged over all elements to obtain a scalar value. Although this general measure of fineness is rather abstract, it has proven useful for outlining how the scale of a microstructure varies across cross-sections.

Figure 2 . Two-dimensional FFT original image, transformation image, weight matrix and weighted results.
Figure 2 . Two-dimensional FFT original image, transformation image, weight matrix and weighted results.

Fineness is drawn by measuring within a 100 × 100 pixel window that is moved incrementally across the panorama. The method was implemented using MATLAB 2021a. In rare cases, artifacts related to panorama stitching can produce systematic patterns in fineness maps. This is solved by adjusting the weight matrix, such as ignoring the shortest few wavelengths in the transformation (shrinkage of the circles in Figure 2c). Figure 3 shows an example of a portion of a fineness map overlaid on an original micrograph, illustrating the correlation between the number of fineness and the apparent fineness of the local graphitic structure. (A smaller window was used for this particular mapping.) To quantify dendrites, the panorama was first segmented, as shown in Figure 4 . The image (Fig. 4a) is first thresholded based on brightness. It was found that it is best to work at a relatively inclusive threshold that is less sensitive to noise within the dendrite arms. The remaining holes smaller than 20 pixels in the dendrite arms were then removed (Figure 4 b). A 6-pixel etch operation is then performed to remove most detail between the dendrite arms, followed by removal of residual objects smaller than 20 pixels (Figure 4 c). The binary image is then smoothed and expanded until the extent of the segmented region is visually consistent with the boundaries of the dendrites in the image (Fig. 4d, e). Smoothing was achieved by filtering with Gaussian blur (standard deviation of 1.5 pixels) and then setting the threshold higher than 0.5 (out of 1). A fineness-based mask is then applied to the segmented dendrites, leaving only regions with appropriate segmentation quality. The position of the masking and boundaries relative to the original micrograph is shown in Figure 4 e.

Figure 3 . Overlay of local graphite fineness. The color scale from purple to yellow indicates an increase in fineness.
Figure 3 . Overlay of local graphite fineness. The color scale from purple to yellow indicates an increase in fineness.
Figure 4 . Threshold segmentation, hole removal, erosion, expansion and masking processes of dendrite images.
Figure 4 . Threshold segmentation, hole removal, erosion, expansion and masking processes of dendrite images.

The segmented panorama was divided into 1 × 1 mm regions of interest (ROI) on which dendrites were measured. The area fraction of a dendrite is measured as the pixel count in the segmented dendrite divided by the pixel count in the measurement area (excluding the masked area). The volume fraction V_V^D is assumed to be equal to the area fraction. Measure the perimeter around the dendrite, excluding the boundaries of the shaded area. Border length was measured by calculating the vertical, horizontal, and diagonal distances along the border and then multiplying by a correction factor of 0.94806 to eliminate overestimation due to the jagged nature of pixelated borders. The surface area per unit volume is then calculated as S_V = 4/π *L/A_m , where L is the perimeter and A m is the measured area, excluding the shaded area. The conversion from perimeter to surface area requires a stereoscopic coefficient of 4/π. The calculation formula of dendrite modulus is M^D = V_V^D /S_V^D. Austenite grain orientation was mapped using an EDAX Trident EBSD system in a Schottky field emission gun electron microscope (Tescan LYRA3) operating at 20 kV in a 1500 × 1700 μm field. The scan step size was 2 µm. The sample surface normal is at an angle of 70° to the beam. The area was mapped into four slightly overlapping quadrants, which were subsequently spliced.

Grain distribution, graphite morphology and dendrite results

The temperature measured at the center and the average of the three temperatures measured at the surface are shown in Figure 5. The cooling curve in the center shows that the casting has various liquidus temperatures, which roughly correlate with the carbon equivalent (CE) calculated from the chemical composition (Table 1) and the liquidus temperature (dashed line) in Figure 5, calculated using Thermo-Calc and the database TCFE13. The liquidus temperature was also compared to calculations using an older version of the database, TCFE7, but this underestimated the liquidus temperature even more than TCFE13. The grain structure is shown in Figure 6. All castings included cylindrical regions and internal equiaxed regions, similar to observations for cylindrical LGI produced in sand molds. The fine-grained structure of the columnar zone and its direct connection to the steel shell indicate that austenite can easily nucleate inside the steel shell (or grow directly from it). This is reasonable because the temperature measured at the outer surface (Fig. 5) exceeds the austenitizing temperature, which means that the steel shell is austenitic when the melt reaches the liquidus temperature. Casting A1 in Figure 6a and Casting B1 in Figure 6b also show a columnar region surrounding the central steel tube; however, its boundary with the equiaxed band is not clear and is therefore not drawn. Furthermore, the equiaxed zone appears to contain a subregion of rather small grain sizes, from here onwards known as the high count zone (HCZ).

Figure 5 . Center and surface cooling curves and Thermo-Calc liquidus; CE=C+(Si+P)/3.
Figure 5 . Center and surface cooling curves and Thermo-Calc liquidus; CE=C+(Si+P)/3.
Figure 6 . Austenite grain diagram and columnar zone-equiaxed zone boundary synthesized from multiple illumination angles.
Figure 6 . Austenite grain diagram and columnar zone-equiaxed zone boundary synthesized from multiple illumination angles.

Grains in the columnar region were quantified in terms of area fraction and volume fraction. The equiaxed zone is quantified as the number of grains per unit area, where both counts and area exclude the HCZ and grains in contact with the steel pipe. HCZ was excluded to better represent the main equiaxed region, which has a much lower grain number. The number of grain structures is shown in Table 2. The area fraction of columnar region A_A^Col ranges from 0.334 in C2 to 0.442 in B1. The columnar area volume fraction V_V^Col is always greater than the area fraction A_A^Col, ranging from 0.438 for A1 to 0.608 for B1. This emphasizes that although the columnar region may appear relatively thin in cross-section, it constitutes a considerable portion of the volume of the spherical casting. The carbon equivalent does not show a significant correlation with the area (or volume) fraction of the columnar zone (A_A^Col, V_V^Col), nor with the number of grains per unit area in the equiaxed zone, N_A^Eq. This is in contrast to findings for ductile iron, where hypereutectic and near-eutectic components exhibit smaller columnar zones and more equiaxed grains than the hypereutectic component. The area fraction of the high-count region A_A^HCZ is largest in C2 and B1, but also exists in B2 and C3. The near-eutectic irons A1 and C1 do not have regions of significant HCZ.

A1 has the most complex graphite structure. Compared to all other castings, it has the coarsest flake graphite structure, showing more branching and intertwined eutectic cells with less clear boundaries. However, fine graphite regions are also distributed in this section and appear bright in Figure 8a. From now on, these zones are called fine graphite zones (FGZ). The FGZs in A1 stand out because they contain significantly finer dendrites than the surrounding structures. Since the size of dendrites grows with local solidification time, this means that the FGZs in A1 correspond to gaps in the early dendrite structure that are later filled by new, finer dendrites. As shown in Figure 9, the dendrites in the FGZ of other castings are not small, but are similar to dendrites embedded in coarser flake graphite regions. Figure 10 shows a close-up of the FGZ surrounded by coarser structures, where the EBSD map of the austenite grain orientation is compared with the electron backscattered image. Interestingly, the FGZ belongs to the same austenite grain as the nearby coarser structures. This suggests that austenite in the FGZ is not independently nucleated but extends from adjacent austenite grains. This is further supported by the fact that the fine dendrite arms found in the FGZ have similar orientations to the larger dendrites in the same grain. The number of non-indexed and blank pixels in the figure is related to the usually finely dispersed graphite and retained austenite (FCC) which only accounts for about half of the ausferite matrix.

Figure 8 . Cross-sectional graphite fineness diagram and eutectic cell distribution.
Figure 8 . Cross-sectional graphite fineness diagram and eutectic cell distribution.
Figure 9 . Comparison of A1 and C1 fine graphite areas.
Figure 9 . Comparison of A1 and C1 fine graphite areas.
Figure 10 . EBSD and backscattering images of the A1 fine graphite region, comparing crystal orientation.
Figure 10 . EBSD and backscattering images of the A1 fine graphite region, comparing crystal orientation.

The reason for the unique FGZ in A1 is unclear, but the fact that it has the highest carbon equivalent in the alloy is suspected to play a significant role. The cooling curve for A1 in Figure 5 shows a continuous re-glow with a single temperature maximum, indicating very limited dendrite growth before the eutectic. The number of primary austenite dendrites is known to decrease as the carbon equivalent increases to the eutectic composition. Although dendrites are also frequently observed in eutectic and hypereutectic LGI, their presence or amount depends more on the cooling rate than in hypoeutectic alloys because they grow in competition with the eutectic. In this sense, before the lap connections, the development of the dendrite structure may have been interrupted due to the interference of the almost simultaneously growing eutectics. Reactivation of dendrite growth may occur later as eutectic growth is slowed and allowed to cool, for example due to impaction of the eutectic cells. Altogether, the complexity of the microstructure in A1 appears to be related to its high carbon equivalent, which leads to disruption of dendrite growth during early solidification before the establishment of a coherent dendrite structure. Gaps in the dendrite framework are filled in later stages of solidification by reactivation of dendrite growth, but scarring is left in the form of significantly finer dendrite patches embedded in finer flake graphite eutectics.

Two castings (B1 and B2) inoculated with Sr-FeSi showed significantly smaller eutectic cells compared to all non-inoculated castings (Fig. 8). The graphite sheet structure is also coarser and more uniform with fewer FGZs in B1 and B2 compared to C1-C3. In contrast to A1, the graphite in B1 and B2 forms roughly rounded coarse graphite eutectic cells, shown as black dots against a lighter background in Figure 8b,c. The bright FGZs in B1 and B2 do not contain finer dendrites, as observed in A1, indicating that dendrite growth is not interrupted before lap connections. This is reasonable because the cooling curves for B1 and B2 in Figure 5 indicate that dendrites have time to develop independently before eutectic growth begins. Dendrites were measured only in casts C1–C3, where dendrites are most clearly outlined by fine graphite structures in the FGZ. Measurements were classified as belonging to the columnar region if more than half of the quantified region of interest (ROI) overlapped with columnar grains. The dendrite integral fraction (V_V^D) is plotted in Figure 15 as a function of distance from the center of the cross section. The distribution of measured values ​​across the cross-section is shown in Figure 16.

A linear regression of the C1 columnar zone measurements (excluding outliers V_V^D < 0.1 ) gives a slope of 0.0448 cm -1 , a standard error of 0.0034 cm -1 (7.64 %), and a t-statistic of 13.2. The explanation for less austenite in the C1 central dendrite may be the higher carbon equivalent (CE = 4.26). Although hypoeutectic and lower than A1, the smaller margin means that dendrite growth independent of the eutectic is shorter in C1 than in C2 and C3. As discussed for casting A1, the volume fraction of dendrites may therefore be more sensitive to local cooling conditions, creating a radial trend. The dendrite modulus, defined as its volume divided by its surface area, is highlighted as a useful indicator of its degree of coarsening. The interpretation of the modulus can be simplified by considering that the modulus of a long cylinder is close to half its radius and that of a sphere is equal to one-third of its radius. The dendrite modulus is plotted against the distance from the center of the cross section in Figure 18. A plot of the corresponding measurement results is shown in Figure 19. Note that measurements in which more than 80% of the area was obscured were excluded, so data points are noticeably missing from the map.

Figure 18 . Dendrite modulus as a function of distance from the center of the casting.
Figure 18 . Dendrite modulus as a function of distance from the center of the casting.

The lower the carbon equivalent, the generally higher the modulus. This is expected because the volume fraction of dendrites increases mainly through the thickening of the dendrite arms after the dendrites reach overlapping connection. In the isometric region, the modulus increases with distance from the surface. This is expected because the center solidifies more slowly than the periphery, allowing the dendrites to coarsen over a longer period of time before being overgrown by the eutectic. However, this trend does not seem to apply to the columnar zone. The break in trend is most obvious in C1, which has the largest column area. The authors currently cannot understand why the modulus does not increase along the columnar dendrites in the same manner as in the equiaxed zone. But if this is the case, it would be feasible to refine the dendrite modulus by promoting columnar growth. As mentioned previously, casts C2 and C3 include areas with anomalous HCZs (observable in Figure 6 ). Figure 20a first shows that each grain appearing in Figure 6 contains a dendrite whose arm orientation is unique to that grain and, as expected, different from its neighboring grains. Furthermore, comparison with Figure 20b shows that the dendrite structure in HCZ is less ordered, as expected for small randomly oriented equiaxed grains. This confirms that the grains (including HCZ) observed in Figure 6 are not artifacts of the austempering treatment or etching process, but truly reflect the austenite grain structure. The volume fraction and modulus of dendrites in the HCZ were not found to deviate significantly from the surrounding dendrite structure, implying that they may have grown more or less synchronously with adjacent large dendrite grains. The fineness plot in Figure 8 also does not show any significant deviation for HCZ in the fineness or size of the eutectic cells. Unless dendrites in the HCZ have coalesced (albeit with different crystallographic orientations), a reduction in continuity in this region is expected. This may be important for feeding behavior and material properties, for example.

Figure 20 . The C1 dendrite segmentation map is superimposed on the grain map, and the coarse grain area and the high grain number area are compared.
Figure 20 . The C1 dendrite segmentation map is superimposed on the grain map, and the coarse grain area and the high grain number area are compared.

The mechanism of action of HCZ is unknown. Heterogeneous nucleation of equiaxed dendrites may be involved, but it is unclear how this leads to a locally higher density of nucleation sites. Dendrite fragments may also be involved. It has been demonstrated that dendrite arm fracture occurs in cast iron under isothermal holding conditions above the eutectic temperature. However, thermal solute convection and solute enrichment associated with decelerating solidification fronts may exacerbate fragmentation. 61

Table 2. Original paper data

Description

symbol

unit

A1

B1

B2

C1

C2

C3

area fraction of columnar area

A_A^Col

[–]

0.357

0.442

0.372

0.433

0.334

0.358

Volume fraction of columnar area*

V_V^Col

[–]

0.438

0.608

0.532

0.588

0.485

0.471

Area fraction of high grain number area

A_A^HCZ

[–]

–

0.052

0.019

–

0.074

0.012

The number of grains per unit area in the equiaxed area (excluding high grain number areas)

N_A^Eq

[m−2]

3.10e5

2.37e5

2.46e5

3.00e5

4.21e5

3.78e5

Source: Domeij, Björn, Diószegi, Attila. Relationships Between Macrostructure and Microstructure in Lamellar Graphite Iron Castings. 2024-04-22. DOI: 10.1007/s40962-024-01319-3. Adapted from the open-access paper; original figure/table numbers retained. CC BY 4.0.Original paper · PDF · CC BY 4.0 ·