Dual-Alloy Sand Casting: Mixing Zones, Chilling and Oxide Inclusions
Published:
2024-03-02
The sequential pouring test of AlSi9Cu3 and AlSi12 combines thermodynamic calculations, mold filling simulation and microscopic analysis to reveal the shape of the mixing zone and the formation conditions of oxidation defects.
Figure 9 . The simulated temperature after waiting for 60 s, as well as the temperature and flow rate when the second inner gate is filled.
Alloy systems, calculations and pouring tests
Thermodynamic equilibrium composition calculations were performed using the Equilibrium module in the HSC Chemistry 10 program. Based on the thermochemical data of enthalpy (H), entropy (S) and heat capacity (C), the Gibbs energy minimization method is used to calculate the multi-component equilibrium composition under non-ideal conditions. Thermodynamic modeling allows estimation of the number and type of components formed when the alloy interacts with air and in an inert argon atmosphere in the temperature range 100–700 °C in steps of 25 °C. Calculations of metallic phases of different compositions were carried out depending on the alloys studied (AlSi12, AlSi9Cu3 and mixed alloys). The chemical composition of the alloy is shown in the table. 1. The dosage of each alloy is 1.25 kg (according to experiment). The gas volume is 0.001Nm 3 (space above the ingot contact surface) of air or argon. The air atmosphere contains 0.0008Nm 3 N 2 and 0.0002Nm 3 O 2 . The thermodynamic system does not include the influence of hydrogen-containing components (H 2 O, H 2 ). Calculation of the equilibrium composition shows the formation of aluminum and magnesium oxides (Al 2 O 3 , MgO, MgAl 2 O 4 ) in an air atmosphere. The total content of these oxides is shown in Figure 2.
The oxides formed in the temperature range 100–700 °C are different for each alloy. However, the central tendencies are similar. The major oxide in all alloys is MgO. Its equilibrium content is the highest among other oxides, especially the AlSi9Cu3 alloy, which has the highest initial Mg content (see Table 1). The change of MgO content with temperature is not important. It increases only slightly over the studied temperature range of AlSi12 and hybrid alloys. According to the Gibbs free energy (Fig. 4a), it can be assumed that in the thermodynamic system of Mg, Al and air (O 2 , N 2 ), aluminum and magnesium oxides are first formed. Al then reacts with N 2 to form AlN inclusions. In 35, it was experimentally determined that when the air in the bubble interacts with the Al-7Si-0.3Mg alloy melt, oxygen is consumed first and then nitrogen. The Gibbs free energy diagram (Fig. 4a) shows the reaction between pure elements and oxides to form spinel (MgAl 2 O 4 ). The reaction of spinel MgAl 2 O 4 due to the reaction between MgO and Al 2 O 3 has a complex transport mechanism that occurs with Mg 2+ ions. Immerse the magnesium oxide in the alumina tube into molten aluminum. The ions Mg 2+ in MgO are reduced by Al near the molten Al/MgAl 2 O 4 interface on the MgO side. The reaction is 4MgO + 2Al = MgAl 2 O 4 + 3Mg. In addition, Mg is dissolved into the molten aluminum. At the molten Al/MgAl 2 O 4 interface on the side of the Al 2 O 3 tube, Mg is oxidized into Mg 2+ ions, and spinel is generated according to the reaction 4Al 2 O 3 + 3Mg = 3 MgAl 2 O 4 + 2Al.
Figure 5 compares the equilibrium contents of Al and Mg in air and argon. In calculations under an argon atmosphere, the absence of oxygen and oxides is assumed. Generally speaking, the contents of Al and Mg in argon gas are higher than those in air atmosphere. The equilibrium content of Mg 2 Si in argon gas is higher than that in air atmosphere. It decreases when the temperature increases (Table 2). Additionally, the magnesium content increases more in argon than in air atmosphere. This process is likely due to active oxidation of magnesium in the air. The amount of Mg 2 Si depends on the initial magnesium content of the alloy. The higher it is, the greater the amount of Mg 2 Si formed. The experimental casting process was simulated using Flow3D Cast v5.0. Simulations were performed with the injector in position I shown in Figure 9 . The simulation is carried out in three sub-processes. The first subprocess simulates the filling of the mold via the first ingate system (1) until the filling level of the melt reaches the second ingate. In the second sub-process, the poured melt solidifies within a specified time, resulting in a semi-solid state in the evaluation geometry (4). In this work, 60 seconds were defined between the start of pouring of the first alloy and pouring through the second ingate system. In the third simulation sub-process, the second melt is poured through the second ingate (2) until the mold is completely filled. The alloy AlSi9Cu3 is used as the casting material, and the pouring temperature is 650°C (inner runner 1) and 640°C (inner runner 2). Differences in thermophysical properties between the melts introduced through the first and second ingates were ignored because the final solidification of the compounds was not studied. The heat transfer coefficient (HTC) between the liquid melt and the mold was set to 800 W/m 2 K and the HTC between the solidifying metal and the mold was set to 200 W/m 2 K. A linear dependence of the solidifying material and temperature in the semi-solid interval (582–521 °C) is defined for this material. The sand mold material is furan resin sand. In the simulation, the melt filled first showed a temperature of approximately 545–558 °C when pouring the second melt started (Fig. 9a). During the second filling process (Fig. 9b), some of the already solidified material is remelted and the two alloys are mixed.
The first experimental sand castings were performed individually for each alloy (AlSi9Cu3, AlSi12) and a mixture of both. The casting of pure alloys takes place through a gate at the bottom. The alloy mixture was produced by pouring 50% of the alloy AlSi9Cu3 through a bottom gate. Twenty-seven seconds after the first batch of alloy was poured, another 50% of the alloy, AlSi12, was poured on top. The studied properties of these castings were used as reference properties for the analysis of bialloy sample ingots with area and mixed zones for each alloy. Further sand casting experiments (Table 5) were performed under different conditions using two alloys (AlSi9Cu3-Alloy 1, AlSi12-Alloy 2) to evaluate the mixing zone between alloys. These experiments were performed to obtain preliminary results that can be used to better understand the multi-material injection casting process for future experiments using injection casting machines (Fig. 1). An illustration of the sand mold, the layout of the casting system, and the location of the ceramic filter and cooling metal plates is shown in Figure 10a. The injector position is modeled by the level of the first alloy, which is poured through the lower ingate above (Position I) or below (Position II) the level of the second ingate. When the liquid level of the first alloy is higher than the second ingate (position I), the insulated tube prevents the second ingate from freezing during the exposure time. Cut a channel approximately 10 mm x 5 mm in the lower part of the second alloy insulated tube. At the bottom of the cavity, steel or sand inserts can be placed into the sand mold (Fig. 10b). The insert reduces the exposure time of the first alloy, minimizes contact with air, and adjusts the direction of solidification during casting. The melt temperature in the furnace is 742 °C for AlSi9Cu3 and 682 °C for AlSi12. The temperature of the first alloy (AlSi9Cu3) was approximately 530 °C when the second alloy was poured when using the steel plate, and approximately 570–580 °C when the second alloy was poured without the steel plate. The resulting casting weighed approximately 0.71 kg (262.4 cm 3 ).

The resulting castings were cut into samples and examined using different methods and equipment. Microstructural analysis of the samples was performed using a reflected light microscope Zeiss Axio Imager M.2 at magnifications of 25×, 50×, 100× and 200×. Spark spectroscopy measurements have been performed to determine the distribution of elements in cast specimens. Samples were cut along the vertical midplane and 15-20 individual locations per sample were studied. Measurements were taken using Foundry Master from WAS/Oxford Instruments. In addition to spark spectroscopy measurements, scanning electron microscopy (SEM) and energy-dispersive X-ray spectroscopy (EDS) were used. A VEGA TESCAN 5130 XL with EDS was used with the following measurement specifications: spot size 68 nm, absorption current 38 pA, voltage 20 kV, working distance 35 mm, detector BE, magnifications 50x, 485x and 1800x. The EDS detector is cooled by nitrogen gas. The following steps were performed: (1) quantitative analysis of rectangular area spectra from top to bottom of the sample, and (2) area and point spectra in possible inclusion and aluminide regions. In quantitative analysis, all elements were present in both alloys. N and O were also analyzed to clarify possible inclusion and pore formation causes.
Compositional transitions, microstructure and defects
The cross-section of the studied casting surface has three zones: alloy 1 (AlSi9Cu3), alloy 2 (AlSi12) and the mixed zone. The samples used for EDS studies were cut from the central part of the casting (Fig. 11). The size of the sample is 50x50mm. The mixing zone is defined by relative contents of elemental copper from 0 to 3.3 wt.% (100% relative content) and from 11 wt.% (0% relative content) to 13 wt.% (100% relative content) of elemental silicon. Alloy samples have different microstructures and therefore should have different mechanical properties: dual primary precipitates, primary α solid solution dendrites, some primary silicon, (α+Si) eutectics and different aluminides. The type of aluminum matrix and the content of primary silicon are different. AlSi9Cu3 alloy has the highest aluminide content due to its high alloy composition, especially copper content. Spark spectrum measurements show that the average Cu content in AlSi9Cu3 is 3.31 wt.% and the average Cu content in the mixed alloy is 1.87 wt.%. The Cu content in the alloy mixture was approximately the same throughout the sample, indicating complete mixing of the two alloys.
Below are the results for dual alloy castings. To identify the mixing zone, we track changes in Cu content measured by spark spectroscopy and EDS. The red line shows the approximate midline (or region) of the mixing zone where Cu changes sharply (Figure 13 a–e). The position of the mixing zone line was also confirmed by microstructural studies (see Figure 14). The condition on the polished surface of the sample can be detected "with the naked eye" at the appropriate angle of light incidence. Figure 13f shows the variation of the average Cu and Si contents with the height of the bialloy ingot. Compared to the assumed mixing zone area (Fig. 11), the copper content averages vary from 3% to 2% and the silicon content from 11.3% to 12.8%, which is very close to the content of these components in the mixed alloy composition (Table 1). The sharp change in Cu in the transition zone is from about 2.5-3.6% to 1-2%. In all cases, the Cu content remains near 1% up to the top of the casting. The casting method affects the contour of the mixing zone (center line). The most horizontal interface was observed in samples I and IV when alloy 2 was cast on top of alloy 1. In this case, different crystallization conditions are compensated by different amounts of Alloy 1. Cast IV contains approximately twice as much alloy 1 as the other castings. Due to the additional cooling and longer waiting time, the crystallization rates of Alloy 1 in castings I and IV are believed to be approximately the same.


If the second alloy is cast when the first alloy is above the second ingate (position I), the interface is deeper on the second ingate side due to more heat contribution. However, the use of cooling (steel) plates results in a smoother profile of the mixing zone. When comparing castings III and V to II, the additional cooling (chill) has a more significant effect on this process than the waiting time (Fig. 12). Therefore, the use of chilling rather than prolonged exposure of the metal can reduce contact time with air and reduce the effects associated with oxide formation. Casting method and bottom cooling affect the mixing zone profile more significantly than exposure time. Table 6 shows the diffusion of other components that are present in one alloy but not in the other alloy. They are Mn, Cr and Zn in the AlSi9Cu3 alloy and Ga in the AlSi12 alloy. The initial contents of these ingredients are shown in Table 1. Due to its specific color, the distribution of copper complexes in the metal structure can be seen. The alloy 1 (AlSi9Cu3) region has a more extensive network of primary Al dendrites. This trend is similar to the microstructure of the individually cast original alloy (see Figure 12).

The obtained component contents indicate the presence of the following compounds based on thermodynamic calculations: Al 3 Ni, FeAl 3 , TiSi 2 , TiSi, MnSi, CrSi 2 , Cu 2 Mg, FeAl 2 , etc. (see Table 4). Some spectra show the presence of iron-rich compounds (see Introduction section). The intermetallic phase also contains some oxygen (0.87–6.35%). As mentioned in the introduction section, one of the causes of pore formation may be non-metallic oxide inclusions. There are many pores in the experimental ingot. There are relatively few pores in samples III and V. The highest porosity is concentrated in the lower part of the ingot and near the mixing zone. EDS studies of porosity showed that many of them contained oxides internally (Fig. 16, Table 8). The data in Table 8 confirm the results of the thermodynamic calculations and indicate the presence of MgAl 2 O 4 , MgO and Al 2 O 3 . Nitrogen corresponding to the compound AlN was identified in both spectra (4, 7). In the microstructure of sample I, a larger oxide film was found in the upper part (Fig. 17a). Oxide inclusions are located inside the primary silicon crystal. Figure 17b shows the same inclusions in sample V.


The study results of EDS spectral points show that the oxygen content is 21.09% (sample IV) and 39.99% (sample IV), indicating that MgAl 2 O 4 or Al 2 O 3 oxide exists in the primary Si crystal. Therefore, it is clear that a certain amount of oxides formed on the surface of Alloy 1 and that these oxides made their way into the metal through the pouring of Alloy 2. Casting conditions will be further investigated to obtain dense, defect-free bialloy ingots. The highest porosity is concentrated in the lower part of the ingot and near the mixing zone. One of the causes of porosity is the formation of non-metallic inclusions (mainly oxides) due to the interaction of the first part of the alloy with air during exposure. EDS analysis of the shrinkage pore surface showed the presence of oxides and nitrogen on its surface, corresponding to MgAl 2 O 4 , MgO, Al 2 O 3 and AlN (also in the thermodynamic simulation).
Test number | Target waiting time (s) | Actual waiting time (s) | Use chill | heat insulation | The first batch of alloy liquid level relative to the position of the second inner gate |
|---|---|---|---|---|---|
I | 60 | 81 | No | Yes | Below (Position II) |
II | 120 | 135 | No | Yes | Higher than (position I) |
III | 60 | 65 | Yes | Yes | Higher than (position I) |
IV | 120 | 124 | Yes | Yes | Below (Position II) |
V | 90 | 94 | Yes | Yes | Higher than (position I) |
Source: Lisova, Liudmyla, Erber, Maximilian, Rottenegger, David, Fuchs, Georg, Braunreuther, Stefan, Volk, Wolfram. Dual-Alloy Sand Mold Casting: Main Principles and Features. 2024-03-02. DOI: 10.1007/s40962-024-01289-6. Adapted from the open-access paper; original figure/table numbers retained. CC BY 4.0.Original paper · PDF · CC BY 4.0 ·
Related News