Gray Iron Filling Systems: Simulation, Production Trials and the Cost of Quality


Published: 

2024-02-09

Taking EN-GJL-250 bearing shell as the object, four gating systems are compared, and air entrainment, flow rate, production scrap rate and quality cost are linked.

Figure 3 . The original pouring system D1, the exhaust structure is omitted in the figure.

Figure 3 . The original pouring system D1, the exhaust structure is omitted in the figure.

Gating system design and production verification method

Production parts were selected that consistently exhibited subcutaneous porosity defects. This part is a 1.57 kg passenger car bearing housing manufactured to grade EN-GJL-250 (see Table 1). The part was manufactured on a high-volume, vertically parted green sand molding machine using a six-cavity mold and contained two shell-shaped sand cores produced with 60 AFS sand at an LOI of 1.6%. The metal is melted through four cold-air coke cupolas and transported via 250 kg transfer ladles to the production line, where it is distributed into unheated pouring units and treated with inoculants - the lack of post-furnace heating results in wide pouring temperature limits in production (1350 °C - 1420 °C). Internal and external scrap rates for the eight months prior to the study were 15.3% and 4.17%, respectively. A Pareto analysis of a sample of 1,000 internal and external defects found that 64% of external defects were related to porosity defects and 71% of internal defects were due to water jacket core rupture. Figure 1 provides a color illustration of the location of part defects on a machined part, and Figure 2 provides a breakdown of porosity at each location in the Pareto sample and shows that water jacket core side 2 exhibits significantly more porosity defects. It is worth noting that the machining allowance in this area is significantly smaller than the water jacket sand core surface 1, and although the sand core has been drilled out, the sand core air pressure is expected to still be high.

Five representative subcutaneous pore waste samples were sent for independent analysis by scanning electron microscopy (SEM). Table 2 shows an image of one of these five samples taken from mold side 2. The report found the presence of slag and sand in all samples and concluded based on conventional wisdom that these were formed when metal oxides reacted with carbon in solution to form CO gas, which floated and became trapped beneath the solidified skin of the castings. The size, shape of the defect and associated slag and sand also fit Campbell's description of a casting with an entrained bubble defect. The existing system used in the production of test parts (Figure 3) uses CAD software for 3D scanning and modeling. This system, referred to in this paper as Design 1 (D1), has six cavities located on two levels designed to be filled simultaneously. Like many systems in the industry, the sprue cup design is an in-line system with a high-mounted filter designed to (i) prevent more prominent inclusions from entering the gate, and (ii) reorganize turbulent flow into laminar flow. 31, 32, 33

Flow simulation analysis was performed using MAGMA5 using a scanning model. The pouring temperature was set at 1380 °C and was derived from the average pouring temperature of historical production data. The simulation uses approximately seven million grid cells. The simulations were limited to fluid flow results and the pouring conditions were set to 90% of the pouring basin in the system without the stopper mechanism. In the case of the plug system, a text file was used to control the opening and closing of the filter simulated plug with a delayed pressure drop. All simulations were performed on a 64-bit Dell workstation with a 3.7GHz processor and 32GB RAM workstation running Magmasoft 5.5.1 2-core license. As a typical simulation analysis, several simulation predictions, namely air entrainment, free surface area, mold erosion, and gate velocity, are used to evaluate system efficacy and provide an overall review of filling turbulence. Each objective is evaluated both qualitatively and quantitatively; for clarity, the quantitative parameters are worth discussing. These five indicators are average air entrainment AAE, maximum air entrainment MAE, free surface area SF-B minus the sprue cup area, mold erosion ME, and maximum flow velocity GV of the inner gate. MAE reflects the severity of local problems, and AAE reflects the overall air entrainment level; larger free surface areas are usually related to splashes, droplets, and turbulent liquid levels. ME is used to identify the location where the molten iron impacts the molding sand. This study uses the default time and speed thresholds of 4.5 s and 2.25 m/s. GV is measured in m/s, focusing on the last narrow channel before the molten iron enters the mold cavity. Therefore, the objective criterion for quantitative analysis is the reduction of AAE, MAE, SF-B, ME, and GV, with equal weight for each. Qualitatively, however, where appropriate, complementary results such as temperature, velocity and pressure can be used to confirm the mechanisms at play. The vector representation is also activated when appropriate to further interrogate the flow direction.

Following the D1 simulation, a new system was designed around a fixed cavity location and its suitability was simulated. Figure 4 illustrates the new system, which is conceptually similar to the system used by Hsu et al. And designed to fill the cavity sequentially from the bottom of the mold, rather than simultaneously. Different from the solutions of Hsu, Takemoto, and Abe, this design keeps the filtering capacity unchanged and uses only one filter. In addition, tapered sprues at the end of the lower horizontal flow channel, initial flush buffers, and swirl traps were included, as several studies have verified that these influence the defined criteria. The available space on the board and the fixed cavity location impose constraints on the geometry of these features, which may affect their optimality. Figure 5 shows the offset sprue cup design, which weighs 3.18 kg and includes a step to minimize shrinkage cavity recirculation around the sprue opening and an undercut to prevent metal from splashing upward out of the basin. Figure 6 shows a drainable sprue cup designed to accommodate the entire pour weight and drain once the plug is removed. The sprue cup is provided with a groove for placing a metal disc plug made of mild steel, which melts after full contact with the molten iron.

Figure 4 . New pouring system D3 with offset sprue cups.
Figure 4 . New pouring system D3 with offset sprue cups.
Figure 5 . Offset sprue cup for D3.
Figure 5 . Offset sprue cup for D3.
Figure 6 . Drainable sprue cup for D4.
Figure 6 . Drainable sprue cup for D4.

Production trials were conducted by applying the new filling system and sprue cups to existing tools and testing them independently without changing any other production parameters. However, production is still allowed to proceed as usual. As we all know, this production environment does not have the strict controls of a laboratory or simulation. Therefore, a statistically significant large sample size was used to ensure confidence. Since the test investigates the frequency of defective parts and both variables are categorical, a chi-square test is appropriate. Using a known scrap level of 4.17% and a potential level after removing pores of 1.6%, the minimum experiment size was 1004 components per trial at a 95% confidence interval for a two-tailed test. Sample size is 1,500 castings for production and logistics efficiency of each design. The rough castings are analyzed by visual inspection of the exterior and endoscopic inspection of the interior geometry, and are then recorded as pass or fail based on existing defect catalogs and standards. Parts were inspected by an inspector responsible for recording all defective parts within 8 months prior to testing. Likewise, customers visually inspect machined parts and record them as pass or fail, classifying failures by location. Pearson's chi-square test was then performed to ensure the statistical validity of the results.

Filling, scrap rate and economic results

Figure 7 shows the air entrainment results for all four designs. The most significant changes occur between D1 and D2, while changes in the sprue cup between D2, D3 and D4 have a negligible impact on the results, which is difficult to assess qualitatively. Of note is the high air entrainment volume in the cyclone collector. This result could be the result of the vortex trap doing its job effectively, or it could be that the vortex itself created the entrainment and trapped it, the simulation results cannot distinguish between these two explanations alone. The pouring time of D2 extended from 8.9 s in D1 to 13.7 s in D2 due to the significant slowdown of the upper cavity as the incoming melt fought against the back pressure developed. Over-opening the channel to increase flow will only hinder attempts to reduce turbulent filling. This slow fill rate causes two problems: first, increased cycle times and therefore potentially increased manufacturing costs, and second, the potential for cold-related defects. Figure 10 shows the melting temperature when D2 is 85% filled and highlights that the cavity is not yet filled; however, the melted area has dropped below the liquidus.

Figure 7 . Air entrainment simulation results of D1, D2, D3 and D4.
Figure 7 . Air entrainment simulation results of D1, D2, D3 and D4.
Figure 10 . D2 The molten iron temperature when the mold is filled to 85%.
Figure 10 . D2 The molten iron temperature when the mold is filled to 85%.

D3 uses an offset gate cup to reduce the flow rate in the sprue, thereby reducing the flow rate in the ingate. However, overall padding adds another 0.3 seconds. It is also worth noting that when filling, trapped air is visible within the gate (0.7-0.9 seconds), indicating that the gate design is not optimal. In contrast, once the plug is released from Design 4 (D4), the sprue, surge, filter, and front half of the downrunner fill quickly without creating isolated air pockets. However, as the sprue cup drains and the ferrostatic height decreases, the filling rate of the upper cavity slows down. Despite this, after deducting the basin filling time (4.5s), the cavity filling time is still equal to D3. In addition to qualitative images, Tables 6, 7, and 8 provide quantitative data for all designs. Applying the same weight to each simulation result, D3 ranks highest (Table 6). Table 7 highlights the percentage change between D1 and D2 for each simulation result and quantifies the effect of the system. All measurements show a decrease except gate speed. Table 8 shows the percentage change from D2 as baseline to D3 and D4, thus quantifying the impact of sprue cup design on each outcome.

Based on the simulation results, D2, D3, and D4 were built and installed into existing tools. However, the D4's sprue cup was found to be hampering the production line's existing clamping mechanism. Although modifications were possible, only D2 and D3 were advanced to the manufacturing stage due to financial and time constraints and taking into account simulation results. D4 therefore only has simulation results and has not completed this production verification. Figure 11 shows the probe temperature during the production of D2 and D3. Temperatures during D2 were more inconsistent than D3, with standard deviations (SD) of 31.6 °C and 13.6 °C, respectively. Furthermore, the probe temperature average is close to the simulated temperature, indicating that there should be a good correlation between the accuracy of the two data sets. When the temperature exceeds the control limit, the core is either removed from the mold or short-cast at shutdown, which is why D2 production times are extended. Probe temperature is not included in the design influence temperature recommendations; instead, as Goodrich emphasized, it may affect porosity results.

Figure 11 . Molten iron temperature measurement records for production tests.
Figure 11 . Molten iron temperature measurement records for production tests.

Figure 12 shows the Pareto chart of the causes of defects by design and cavity. Results from both trials showed a significant reduction in internal scrap, an unexpected result since the system was not designed to improve this metric. Despite the concerns raised by the simulation in Figure 10 and the good correlation between simulated and actual pouring times and temperatures, no cold-related defects in the castings were found in either test. Cross-tabulation of the chi-square test found a significant association between sprue system design and internal scrap χ²(1) = 85.747, p < 0.001. The odds ratio shows that the odds ratio of D1 in producing in-factory waste is 2.5 times that of D2. Since the sample sizes vary and the data for D1 are drawn from a pre-existing group, a Bayesian test is not appropriate. The following hypothesis tests whether sprue cup variation (D2 vs. D3) is statistically related to scrap rate. Chi-square results found no significant association between sprue cup design and in-plant scrap rate χ²(1) = .767, p = 0.381. The Bayesian test provides strong evidence for the null hypothesis BF₀₁ = 28.856.

Figure 12 . Distribution of causes of scrap in the factory for each design and A-F cavities.
Figure 12 . Distribution of causes of scrap in the factory for each design and A-F cavities.

Table 10 lists the external scrap for D1, D2, and D3. Figure 13 provides defect locations shown as a percentage of the total for each design. While both D2 and D3 perform better than D1, D2 performs better than D3, which is in contrast to the literature and simulation results. The chi-square results support the alternative hypothesis in Test 3, finding a significant association between sprue system design and external scrap rate χ²(1) = 12.594, p < 0.001. The odds ratio shows that the odds ratio of D1 in producing processing waste is 1.8 times that of D2. The chi-square test for Test 4 does not support the alternative hypothesis and shows that there is no association between sprue cup design and customer machining scrap rate χ²(1) = 2.221, p = 0.136. As with Test 2, the Bayesian test provides strong evidence for the null hypothesis BF₀₁ = 21.403. Figure 14 shows the total manufacturing cost for each proposal for reducing the external scrap rate, which stops at 1.6% since this is the theoretical limit to eliminate all pore-related defects during machining. The breakeven scrap values ​​for w are 3.9% of D2, 4% of D3, and 3.8% of D4. It was also found that under the given conditions of the model, the direct manufacturing cost COM can increase by up to 33%. After exceeding this range, the economic incentive to switch from D1 disappears.

Figure 13 . The location and proportion of processing defects in each design.
Figure 13 . The location and proportion of processing defects in each design.
Figure 14 . Quality cost comparison of four options.
Figure 14 . Quality cost comparison of four options.

Using the data obtained during the trials, Table 12 lists the parts required, the COQ for the proven quality performance, the tonnage required, and the associated environmental impacts. The potential financial savings from switching from D1 to D2 is $94,323. The estimated carbon dioxide emission reduction for the same scenario conversion is 3 tons. However, 7 tons can be saved using D3 due to improved process yield. Smooth charging also resulted in unexpected internal scrapping results. There was no intention to reduce the occurrence of water jacket core ruptures with the new system; however, it resulted in a 57% reduction in internal scrap performance. Statistical analysis rejected the suggestion of random association, and D3 achieved a similar reduction. Qualitative review of the simulation results after the test highlighted differences in filling speed around the gate (Fig. 15). Notably, the metal jet in D1 is dampened by the water-jacketed core it strikes. Additionally, stress simulations performed by the software manufacturer provided evidence that the new system reduced mechanical and thermal stresses on the water jacket core legs during the filling cycle (Figure 16).

Figure 15 . Filling flow rate of D1 and D3.
Figure 15 . Filling flow rate of D1 and D3.
Figure 16 . Water jacket core stress during D1 and D2 filling, the green circle is the damaged location.
Figure 16 . Water jacket core stress during D1 and D2 filling, the green circle is the damaged location.

While it is helpful to use the model to quickly assess the economic efficiency of quality versus cost, the proven savings calculated from the model are more important to the organization. Financial and environmental performance show that significant savings can be achieved by improving quality even as initial manufacturing costs increase. In the best-performing trial, D2, annual savings of $94,323 and a reduction of 3 tons of CO 2 emissions were estimated, despite increases in direct manufacturing costs and total pour weight per box. These numbers highlight the short-sightedness of considering only consumable cost and process yield per case when reviewing system design, and demonstrate that quality-focused gating systems are also the most cost-effective and environmentally friendly systems. Considering the direction of future work, the new pouring concept is a fundamental change and the proposed system is only a first attempt. Further refinement could remove the large, randomly distributed inclusions seen in the experiments. However, the authors believe that even with advanced systems, the porosity around the water jacket core surface 2 is highly sensitive to process control and may always exhibit randomness. Guidance on the optimal dimensions of the initial flush buffer structure and cyclone trap is needed to ensure that a system of this nature maintains reasonable process throughput. Additionally, similar testing on parts prone to cold defects or where fill time determines productivity would further strengthen the findings of this article or provide bounds on their applicability. Finally, the drainable sprue cup concept has great potential and deserves to be tested in the real world. This method not only has the potential to improve quality, but also provides excellent yields and increases productivity.

Table 9. Original paper data

Casting

D1

D2

D3

total

215,176

1475

1499

Qualified

181,953

1376

1386

scrap

33,233

99

113

Scrap rate

15.44%

6.71%

7.54%

Table 10. Original paper data

Casting

D1

D2

D3

total

Qualified

174,367

1345

1342

175,712

scrap

7586

31

44

7,617

total

181,953

1376

1386

183,329

Scrap rate

4.17%

2.25%

3.17%

 

Source: Heyworth, Robert. The Influence of Filling System Design on Quality Performance in Gray Iron. 2024-02-09. DOI: 10.1007/s40962-024-01264-1. Adapted from the open-access paper; original figure/table numbers retained. CC BY 4.0.Original paper · PDF · CC BY 4.0 ·