Molten Iron Penetration into Sand Molds: The Role of Capillary Pressure and Pore Structure


Published: 

2023-10-26

The penetration depth under varying sulfur content and static pressure was investigated using a stepped-cone test; an equivalent aperture slope was introduced, and a heat‑flow coupling simulation was employed to analyze the mechanism underlying the cessation of penetration.

Figure 1 . A schematic illustration of the experimental setup with dimensions in millimeters.

Figure 1 . A schematic illustration of the experimental setup with dimensions in millimeters.

Permeability Testing and the Equivalent Aperture Model

The penetration experiments to investigate the penetration depth were performed by using the so-called step-cone casting method, which is shown in Figure 1 . The step-cone specimen casting is widely used in foundry scale tests for the evaluation of veining and penetration tendency quantitatively. Both the mold and the step cone core were made using a standard quartz sand aggregate bonded with a furan resin-based binder system. The core mixture was produced using various levels of sulfur additions (0, 1, 1.5 and 2 mass%). The various sulfur addition is denoted as S0, S1, S1.5 and S2. Sulfur being a surface-active element was added to study its influence on the penetration depth of molten metal between the sand grain interspaces. The molten metal was a cast iron alloy of eutectic composition 3.59%C, 0.32%Mn, 2.51%Si, 0.015%S, 0.032% P and 0.06%Mg in mass%, and it was cast into the mold with a pouring temperature of 1380 °C. Penetration depth at different heights of the step cone with various sulfur levels was examined using an optical microscope.

Results of Model Verification and Thermal-Hydraulic Coupling

The penetration depth of molten cast iron into the sand core at each level is summarized in Table 1 . According to Figure 1 , the average depth of Level 1, H , is 12.5mm and the density of the molten cast iron, ρ , is 6914 kg m^ - 3 and thus the metallostatic pressure P_M at Level 1 can be calculated as P_M = ρ gH = 6914 × 9.8 × ( 12.5 × 10^ - 3 ) = 847 Pa. The metallostatic pressure at other levels can also be calculated in the same way. The metallostatic pressure at each level is summarized in Table 2 . The penetration depth at each level is plotted as the function of the metallostatic pressure together with linear fittings (Figure 2 ). The contact angle θ (Figure 3 ) should be larger than 90 ^° because, according to the experimental results (Table 1 ), the penetration depth increases with increasing the sulfur amount in the core at the same level, i.e., the same metallostatic pressure. Increasing the sulfur amount in the core corresponds to decreasing of the surface tension σ of the penetrating molten cast iron. The influence of the sulfur on the contact angle is ignored since there are no reliable data and estimation method. Under such conditions, if the contact angle is smaller than 90 ^° , the penetration will be suppressed with decreasing of surface tension because in the case of θ < 90 ^° , the pressure (2σ cos θ )/(r) acts to promote the penetration. According to the result of S0 in Figure 2 , the penetration starts at P_M = 671 Pa. On the other hand, the penetration of the molten metal into porous oxide such as sand mold, i.e., when the contact angle is greater than 90°, the penetration will take place when P_ex > (2σ cos θ )/(r) according to Washburn’s equation, where P_ex is the external pressure including the metallostatic pressure at the molten metal–porous media (sand mold) interface, σ is the surface tension of penetrating molten metal, θ is the contact angle between the molten metal and porous media (sand mold) and r is the pore radius. From Figure 4 , the maximum pore radius, r_max , is estimated as 100 μm and the contact angle, θ , and the surface tension, σ estimated as 120° and 1.7 N m^ - 1 , respectively (estimated based on the literature data ). Then, the required external pressure for the penetration, P_ex , can be calculated as 17,000 Pa. This is a total external pressure which includes the metallostatic pressure, i.e., 671 Pa out of 17,000 Pa is the metallostatic pressure, and the rest of the pressure is the contribution of dynamic pressure and expansion pressure that act so as to promote the penetration, and gas pressure in the mold (pores) and friction pressure that act so as to suppress the penetration. Among these pressures, the dynamic pressure is negligible in the present system since, as shown in Figure 1 , there is no direct impingement of the melt to the sand core wall. The maximum gas pressure is estimated as ca. 700 Pa. The friction pressure is negligible in the case of a shorter penetration depth like the present results. According to Lee and Kayama, the expansion pressure of cast iron during the solidification reaches maximum ca. 5 MPa when the free surface area is minimized. Therefore, the expansion pressure can be a dominant factor.

Figure 2 . Metallostatic pressure dependence of the penetration depth.
Figure 2 . Metallostatic pressure dependence of the penetration depth.
Figure 4 . Microstructure of metal-sand core interface.
Figure 4 . Microstructure of metal-sand core interface.

Based on the above estimation of the total external pressure, by assuming that the pressures other than metallostatic pressure are the same at all levels, the penetration depth is plotted against the total external pressure (Figure 5 ). Regarding the results for S1, S1.5 and S2, it is reasonable to think that the surface tension of the penetrating molten cast iron is reduced due to the adsorption of sulfur. By extrapolating the fitting lines towards h =0 as shown in Figure 5 , the required external pressure for the penetration, i.e., the critical external pressure, P_ex,c , can be obtained for each case, and the surface tension for each case can be calculated using Eqn.(1) where r_max is 100 μm and θ is 120°.

Pex,c=2σcosθrmax(1)

The corresponding surface tension becomes 1.27, 1.07 and 0.9 N m^ - 1 for S1, S1.5 and S2, respectively. In the case of Fe–S binary system, the surface tension decreases from 1.8 to 0.8 N m^ - 1 with increasing sulfur content at 10–60 K above the melting point, and thus the above calculation results are reasonable, and in the case of S2, the surface of the molten cast iron (the penetration front) is almost saturated by sulfur immediately. In the case of the porous medium, which consists of grains, the equivalent capillary radius, r_e , is often used to analyze penetration using the capillary model, and in most cases, a single constant value of r_e is used for the specific porous medium as a parameter that represents the structure of the porous medium. In this case, as explained above, once the penetration starts (i.e., once P_ex > (2σ cos θ )/(r) is established), the penetration will not stop in the case of the penetration in the horizontal direction. However, as explained below, the equivalent capillary radius r_e should not be constant and it should decrease with the penetration depth/height.

Figure 6 shows a schematic illustration of the penetration paths, which have different radii and penetration heights. The penetration takes place from the bottom to the top in the figure. For example, when a slightly higher external pressure than critical pressure ( P_ex,c ) for the radius r_3 is given, the molten metal will penetrate the pores whose radius is larger than r_3 , and the molten metal will penetrate until it meets the pore whose radius is smaller than r_3 . The depth at this point is the maximum penetration depth under the given external pressure. It implies that the maximum penetration depth depends on how long the pore (penetration path), which radius is larger than r_3 , is continuously connected from the bulk part of the molten metal. Now, we may consider a condition in which molten metal is subjected to a pressure that allows it to penetrate into pores with a radius equal to or bigger than r_3 . When the molten metal reached height 2, some of the pores become smaller than r_3 and the equivalent radius also becomes smaller accordingly. The pores whose radius are larger than r_3 may exist at this height (e.g., the pore marked as ‘A’ in Figure 6 ), but such pores will not be counted for the equivalent radius because it is not connected to the bulk part of the molten metal with the continuous pores, which are larger than r_3 . If it is assumed that the different size of pores is randomly distributed in the porous media, the equivalent radius will become smaller and smaller with increasing depth (height), and finally, the equivalent radius becomes smaller than the critical radius, r_cr = 2σ cos θ /P_ex , and the penetration of the molten metal will be stopped. Therefore, it is reasonable to think that the equivalent radius becomes smaller with penetration depth.

Figure 6 . A schematic illustration of various penetration paths ( r 1 < r 2 < r 3 < r 4 ).
Figure 6 . A schematic illustration of various penetration paths ( r 1 < r 2 < r 3 < r 4 ).

Now, for simplicity, it will be assumed that the equivalent radius, r_e , linearly decreases with the penetration depth, h . Then, the equivalent radius, r_e , can be described as Eqn. ( 2 ):

re=rmax−εh(2)

where the slope ε might be called the ‘equivalent radius slope,’ and it is a factor to describe the porous structure. In Eqn. ( 2 ), r_max is the maximum pore radius, and it can be assumed that the maximum pore exists at the surface of the porous media (at the interface between porous media and molten metal). Then, Washburn’s equation can be rewritten as Eqn. ( 3 ):

v=dhdt=(rmax−εh)28ηh(Pex+2σcosθrmax−εh)(3)

The maximum penetration depth, h_max is the depth, h , when Eqn. ( 4 ) is satisfied.

Pex=|2σcosθrmax−εh|(4)
hmax=1ε(rmax+2σcosθPex)(5)

Using Eqn. ( 5 ) and the experimental results, i.e., the relationship between the external pressure and the penetration depth, the coefficient ε at each total external pressure, P_ex , can be calculated. The calculation results of ε are shown in Table 3 . It was found that the value of ε is proportional to the external pressure, P_ex , and σ cos θ , i.e., the thermophysical properties of the penetrating metal ( σ ) and the combination of the penetrating metal and porous media material ( θ ) , and thus the following equation was obtained by multiple regression analysis (the result for S =0 at 17,176 Pa ( ε =0.0068) was treated as an outlier).

ε=0.0215−0.0299×σcosθ−8.77×10−7Pex(6)

The ε value plane obtained from Eqn. ( 6 ) is plotted in Figure 7 , together with the experimental ε values at each condition. By substituting Eqn. ( 6 ) for ε in Eqn. ( 5 ), the maximum penetration depth can be described as follows.

hmax=10.0215−0.0299×σcosθ−8.77×10−7Pex(rmax−2σcos(180∘−θ)Pex)(7)

The calculated maximum penetration depth by Eqn. ( 7 ) and the experimental penetration depth values are plotted in Figure 8 . As can be seen from Figure 8 and Eqn. ( 7 ), in the region where the σ cos θ is relatively high and P_ex is relatively low (the bottom right of the figure), the penetration does not occur. On the other hand, in the region where the σ cos θ is relatively small and P_ex is relatively high (the top left of the figure), the penetration depth changes drastically with σ cos θ and P_ex . The experimental values and the calculated value by Eqn. ( 7 ) are replotted as a function of external pressure in Figure 9 to show the deviation from the calculated values clearly. In the above analysis, the equation for ε (Eqn. ( 6 )) was obtained using all the experimental data. However, the equation can be obtained with enough accuracy from three data points (the plane in Figure 7 can be defined by three points). As a trial, the equation for ε was derived using the three data points provided in Table 4 .

Figure 8 . Measured penetration depth (dots) and calculated penetration depth (grid surface) of molten cast iron.
Figure 8 . Measured penetration depth (dots) and calculated penetration depth (grid surface) of molten cast iron.
Figure 9 . Calculated (curves) and experimental (markers) penetration depth versus the total external pressure.
Figure 9 . Calculated (curves) and experimental (markers) penetration depth versus the total external pressure.

Then, the following equation, which is quite close to Eqn. ( 6 ), was obtained.

ε=0.0215−0.0201×σcosθ−6.56×10−7Pex(8)

The ε value plane calculated from Eqn. ( 8 ) is plotted in Figure 10 together with the measured ε values at each condition. As can be seen from Figure 10 , even employing three data points, the equation for ε can be obtained with a sufficient accuracy. Therefore, it should be possible to evaluate the structure of porous media, i.e., obtain the ε value, by testing the penetration events with three different conditions, and it can be practically used to evaluate penetration in the porous media structure.

In this section, the effect of pore radius change given by Eqn. ( 2 ) on the melt penetration depth and speed is analyzed by computer simulation. The suggested finite element model makes further steps to address the penetration phenomenon complexity, as compared to the developed penetration theory. Inclusion of heat transfer and thus temperature-dependent material properties of cast iron in the finite element model serves to demonstrate that the combined thermal and capillary effects on the melt penetration can only be analyzed by computer simulation, while the presented analytical model considers only pressure balance as the condition to stop the melt penetration. It is worth to investigate by simulation the situations when the hot liquid metal quickly advances through the colder sand mold and the penetration front might cool down to solidus temperature before the pressure balance in the pores is reached or the skin is formed on the mold-metal interface thereby preventing the penetration. In the model, the cast iron penetration depth depends on the pressure balance between the external pressure and the capillary pressure in the pores of the sand mold. On the metal side, the external pressure is assumed to represent a static pressure on the liquid metal side. In the proposed simplified model, it is assumed to be constant, for demonstration purposes. The study is focused on the case of penetration of molten metal into the oxide porous medium (sand mold), i.e., the contact angle is greater than 90°, and therefore, the capillary pressure opposes the metal penetration in the sand mold.

The numerical model was built in COMSOL Multiphysics 5.6, using heat transfer and CFD modules. The model structure is shown in Figure 13 . The model features the multi-physics coupling between the Darcy’s law and phase transport in porous media interfaces to realize Darcy’s law for multiphase flow. The model realizes the local thermal non-equilibrium, enabling the interstitial heat exchange between the sand grains and the fluid represented by two phases: the molten cast iron and the air. The two-dimensional model represented the vertical slice of a sand mold of 10 cm height with symmetry boundary conditions on the sides, and the interface with metal is located on the upper side of the mold, with respect to the gravity, which is pointing in the positive y-direction, as shown in Figure 14 a. Heat fluxes on the metal and the air sides are determined by the respective heat transfer coefficients, transfer coefficients. External over-pressure is applied on the metal side and the mold itself is places in the atmospheric pressure conditions. The heat exchange between the sand grains and the fluids is realized via interstitial heat transfer coefficients. The dense mesh on the metal side is applied to resolve the steep saturation gradient in the initial phase of the computation, as shown in Figure 14 b.

Figure 13 . Model structure and multi-physics interaction.
Figure 13 . Model structure and multi-physics interaction.
Figure 14 . Boundary and initial conditions, and the capillary pressure equation applied in the 2-D model (a); and the meshed geometry.
Figure 14 . Boundary and initial conditions, and the capillary pressure equation applied in the 2-D model (a); and the meshed geometry.

The capillary pressure model includes the temperature-dependent surface tension, iron-sand contact angle and the variable pore radius, R c . The two pore geometries were simulated: straight and tapered, as shown in Figure 15 . The material properties and modeling parameters are summarized in Figures 16 and 17 and Table 5 . Temperature-dependent thermal properties of the mold matrix (solid) were derived from the effective thermal conductivity and specific heat capacity provided in Figure 17 and the respective properties of the air in the pores, based on the mold porosity. For realization of the local thermal non-equilibrium between the fluid and the sand grains, a correlation for the interstitial heat transfer coefficient (IHTC), q_sf , was applied in the spherical pellet bed configuration, Eqn. ( 10 ), as follows:

Figure 15 . Simulated pore geometry: straight pore (a) and tapered pore (b).
Figure 15 . Simulated pore geometry: straight pore (a) and tapered pore (b).
qsf=asf·hsf(10)

where the specific area for the case of bed packed with spherical particles of radius r_p =150 μm is a_sf = (6θ_s )/(2r_p ) , and θ_s = 1 - φ . The heat transfer coefficient in W m −2 K −1 , is calculated as h_sf = ( (2r_p )/(k_f Nu) + (2r_p )/(β k_s ) )^ - 1 where β = 10 for spherical particles, and the fluid-to-solid Nusselt number, Nu , is assumed to approach 1, since the slow process of melt penetration is dominated by thermal conduction, where k_f and k_s are the thermal conductivities of the solid and fluid phases. The simulation results demonstrate two possible situations. If the decrease of the effective pore size is not considered, the penetration speed will become relatively high due to the lower capillary pressure, and the temperature of the mold is relatively low at the penetration front. Hence, as shown in Figure 18 , the penetration might be stopped by the solidification before the pressure balance is achieved. However, as discussed in the previous sections, as the depth of penetration increases, the effective pore radius should be decreased. As shown in Figure 19 , if the decrease of the effective pore size is considered, the penetration speed becomes relatively slow and the temperature at the penetration front becomes relatively high. In this case, the penetration is stopped by the pressure balance, i.e., the metal is still in fully molten state ( T front = 1285 °C) when the metal reached the maximum penetration depth. In other words, the penetration is not stopped by solidification. The stop condition depends, of course, on the value of ε shown in Figure 10 , which is introduced in the previous section. However, the simulation results with typical thermophysical properties and ε value for cast iron and sand mold (Figure 19 ) show that it is possible to stop melt penetration by the pressure balance.

Figure 18 . Straight pore case: metal volume fraction (a) and metal temperature (b) in the mold after 0.7 sec, at the penetration front solidus temperature T front = 1150 °C.
Figure 18 . Straight pore case: metal volume fraction (a) and metal temperature (b) in the mold after 0.7 sec, at the penetration front solidus temperature T front = 1150 °C.
Figure 19 . Tapered pore case: metal volume fraction (a) and metal temperature (b) in the mold after 4.3 sec, at the penetration front temperature T front = 1285 °C, when the pressure balance is achieved
Figure 19 . Tapered pore case: metal volume fraction (a) and metal temperature (b) in the mold after 4.3 sec, at the penetration front temperature T front = 1285 °C, when the pressure balance is achieved

By analyzing the horizontal penetration depth of the molten cast iron into the sand core using the capillary model, the following conclusion was obtained. To describe the influence of the porous media structure and change in the equivalent pore radius on the penetration depth, the equivalent radius slope, ε , is introduced. To obtain ε value was suggested as a novel evaluation method of the porous structure in relation to the penetration. The ε value can be obtained by running the penetration tests with the materials which has different σ cos θ and applying a different external pressure, P_ex . By introducing the concept of the equivalent radius slope, the penetration depth could be reasonably explained as a function of the external pressure and σ cos θ . The penetration height of the mercury and molten steel was also analyzed using the present model, and it was concluded that even for the penetration upwards, at the early stage of the penetration, the penetration might be stopped not by gravity but by the increasing the critical pressure.

Based on the analysis of the maximum penetration depth of molten cast iron, it was concluded that the penetration is not stopped by the solidification since if it is assumed that the penetration is stopped by the solidification, one cannot explain the experimental results on the penetration depth. The penetration will be stopped by the decreasing of the equivalent pore radius, which corresponds to the increasing the pressure which is required for the penetration of θ > 90^° case. The finite element model of liquid iron penetration in a porous sand mold accounted for the complex combination of the capillary effects and heat transfer between the molten metal and the sand mold confirmed that for the selected tapered pore geometry, the penetration was stopped by the pressure balance rather than by solidified frontier of the penetrating melt. The finite element model can be used by process designers for detailed investigation of the early melt penetration at different pore geometries, wetting angles, metallostatic pressure conditions and temperature-dependent thermophysical properties.

Table 1. Depth of Penetration in Each Level

Level

Depth of penetration, mm

S0

S1

S1.5

S2

1

0.15

1.03

1.77

2.47

2

0.35

1.33

2.26

2.68

3

0.53

1.73

2.63

3.28

4

0.72

2.12

3.07

3.63

5

1.10

2.50

3.42

4.02

6

1.58

2.93

4.12

4.73

7

1.83

3.20

4.53

5.32

Table 5. Modeling Parameters

Property/parameter

Symbol, units

Value/expression

Mold height

L0, m

0.1

Mold slice width

W0, m

L0/8

Surface tension, iron31

σ, N m-1

1.725 (no temperature dependence in the temperature range of the present study)

Contact angle

θ, o

120 deg

Capillar pressure, Pa

pc, Pa

2⋅σ(T)⋅cos(θ)/Rc

Mold porosity

φ

0.4

Mold permeability

κ, m2

1.95E-12

Air density

ρair, kg⋅m-3

1.0

Dynamic viscosity, air

μair, Pa⋅s

1.76E-5

Metal static pressure

Pm, Pa

20000.0

Density of sand grains

ρsilica, kg⋅m-3

2640

IHTC, melt-to-sand

qsf,m, W⋅m-3⋅K-1

3.33E+08

IHTC, air-to-sand

qsf,air, W⋅m-3⋅K-1

3.23E+06

HTC, air-to-mold

hair, W⋅m-2⋅K-1

15.0

HTC, metal-to-mold

hm, W⋅m-2⋅K-1

100000*

Melt temperature

Tmelt, °C

1380.0

Solidus temperature, iron

Tsol, °C

1150.0

Initial temperature, mold

Tini, °C

35.0

Matsushita, Taishi, Belov, Ilja, Svidró, József Tamás, Svidró, Judit, Diószegi, Attila. Analysis of the Penetration Behavior of Molten Cast Iron into the Sand Mold. DOI: 10.1007/s40962-023-01169-5. CC BY 4.0。 Original paper · PDF · CC BY 4.0 ·