Austempered Ductile Iron: How Does Austenite Stability Affect Dry Turning?
Published:
2023-06-07
The machinability of three isothermal quenching microstructures was evaluated based on cutting force, martensite transformation, tool wear, surface roughness, and chip morphology.
Figure 1 . Cutting plane from the ADI bars.
Heat treatment and dry turning test
A 100-kg medium-frequency induction furnace was used to melt pig iron and steel scrap with carburizer (99% C), FeSi (65% Si), FeMo (70% Mo) and pure Cu. After deslagging, spheroidization and inoculation were performed at 1520 °C using Fe–Si–Mg alloy containing 9.0% Mg and commercial FeSi inoculant containing 75% Si. The treated iron was poured into green sand molds to make 90-mm-diameter machinability bars and cooled to room temperature. Chemical composition was measured with an Oxford FOUNDRY-MASTER Pro spectrometer.
Several austempering cycles were carried out to produce different ADI and IADI alloys. The heat treatment cycle starts with austenitizing the DI ingots in a controlled environment electric resistance furnace to prevent scaling and decarburization and then quenching in a salt bath furnace where they were held for the duration of the isothermal austempering reaction. Table 2 shows various heat treatment parameters used throughout this work. Light and electron microscope, and X-ray diffraction (XRD) were selected to examine and identify the microstructure constituents of the ADI ingots. For microstructural examination, research samples were ground, polished, and etched using 3% Nital solution. Nodule count and nodularity were calculated using an image analyzer software, ZEISS. When analyzing a metal or alloy with a multi-grain microstructure, color metallography is useful because it highlights different phases or grains that make up the system in contrasting colors. The heat tinting process involves heating the etched samples for 4–8 h in a furnace kept at 260 °C before allowing the samples to naturally cool down to ambient temperature at air.
The processes in sample preparation for the XRD analysis included cutting samples to 25 × 25 × 2.5 (mm) 3 and polishing the surface. The prepared sample was then subjected to XRD analysis on a diffractometer using CuKα radiation ( λ = 0.15406, 40 KV, and 30 MA). The measurements were done in the angle (2 θ ) range between 20° and 104.92° at the rate of 5 s/step. The data obtained are presented as a graph with the angle of reflection (2 θ ) on the abscissa and intensity of the x-rayon the ordinate. The wt% of all phases extracted from the XRD data were calculated measured Reitveld method using MAUD software. The XRD data under consideration by MAUD lie between angles (2θ) 35° to 100°. The main objective of the machinability measurements is to study the impact of machining settings on three different heat treatment cycles-producing ADI grades. Three machinability indicators were used: cutting force, tool wear, and surface roughness. The machining process variables and the experimental design for the machinability trials of this work are shown in Table 3 . The interaction of the various machining factors, such as depth of cut and cutting speed, was explored in relation to the TRIP phenomenon (Transformation Induced Plasticity), which results from the deformation strains caused by machining converting retained austenite into martensite. ADI specimens in cylindrical form underwent single-point continuous turning throughout the machining tests. The workpiece bars had a diameter of 90 mm and were 500 mm in length. The SUS-63-TOZ universal centre lathe was used to conduct the experiment trials. Cutting force analysis and surface roughness analysis were used to assess the machinability of grades ADI 900-375, ADI 900-275, and IADI 820-300. During turning operations, no cutting fluid was applied. To evaluate the role of TRIP phenomena in the ADI samples after the machining, XRD and metallographic samples were cut from the bar using an EDM machine as shown in Figure 1 .
Two different cutting tools were used. The first tool was a CVD-coated carbide, consisting of a smooth, wear-resistant coating, and hard substrates insert TiCN + Al 2 O 3 + TiN). The second tool was a CBN (cubic boron nitride), which is the second only to diamond in hardness. CBN is a synthetically high-hardness material for superior wear resistance and long tool life. The typical application for CBN tools is high-speed cutting which is applicable to heat-treated steel and cast iron. All inserts were clamped on tool holders PCLNR 2525M 12. Table 4 shows the tool geometry of the CVD and CBN inserts used in this study. The cutting force data were measured using a three-dimensional force dynamometer of type 9255B (Kistler, Coherent). The dynamometer accurately measures forces in the x , y , and z axes using the charge generated by quartz crystals. The Kistler charge amplifier type 5814B1 was used to receive the created charge, which is converted into an analog signal and outputs the appropriate force using the computer’s data acquisition card. Using KISTLER DynoWare software (2825A (5697A1)), the generated data were refined and presented in tabular and graphical form. Additionally, the dynamometer was calibrated under static circumstances with defined weights. A Mahr Marsurf PS10 surface roughness tester was used to determine the surface roughness Ra of the ingots.
Phase transformation, cutting force and tool wear
The microstructure of the base ductile iron consists of well-spheroidized graphite dispersed in a mixture of pearlite and ferrite matrix. Alloyed DI with 0.5% Cu and 1% Ni, which are known to be fairly strong pearlite-stabilizing elements, results in 68.4% pearlite in the matrix and limits the ferrite content to 21.7 % in the form of a thin halo around the graphite spheroids as shown in Figure 2 . The graphite morphology was measured in terms of nodule count and sphericity. The nodule count was measured at 172 nodules per mm 2 and a sphericity rating of 81.86%. The graphite spheroids are dispersed in a matrix of extremely fine ausferrite as seen in Figure 3 a as a result of higher rate of ferrite nucleation at higher degree of undercooling, and thus, a more refined ausferritic structure was formed by performing the austempering heat treatment at a lower temperature of 275 °C. The austenite phase appears as white areas, while the ferrite phase looks like dark patches. The ausferrite created from the parent austenite becomes coarser when the austempering temperature is raised to 375 °C, and the higher C-diffusion rate causes the development of coarser ferrite with feathery morphologies, as illustrated in Figure 3 b. Ausferrite and pro-eutectoid ferritic islands make up the microstructure of ductile iron that has undergone intercritical austenitization. The austenite has a relatively low carbon content due to the low austenitizing temperature, which elevates the Ms temperature during air quenching and causes more martensite to develop in the IADI alloy, as shown in Figure 3 c. The microstructure phase analysis of the developed DI and ADI alloys is summarized in Table 5 .

The XRD data for all machinability test specimens were received by Reitveld method using Origin software. The software allows for the automatic background installation and peak fitting of the XRD data against the peak data for selected microstructural phases such as graphite, ferrite, and martensite. The graphite contents measured by the image analysis were remarkably close to each other; therefore, the graphite contents were assumed to be identical for all the investigated samples. In Figure 4 , the XRD peaks represent austenite (γ), ferrite (α), and martensite (M) at various unit cells in the crystal structure. The austenite content is maximum in the ADI-375 alloy (about 35.50 %), whereas low austempering temperature of ADI-275 resulted in a considerable reduction of austenite to around 11%. A rather low austenite content was found in the IADI (about 5%) coupled with rather high ferrite-content of (around 85%). The analysis of martensite contents revealed some interesting values. A minimum amount of martensite was detected in the ADI 900-375; at such relatively high austempering temperature, the C-diffusion rate is rather high, which leads to more stabilized austenite due to its high C-content. The martensite content in the other two samples was similar (approx. 10%), but the martensite formation mechanism in ADI-275 seems to be different. At low temperatures, the slow C-diffusion at such temperature will not be sufficient to ensure complete stabilization of austenite, and the un-stabilized austenite will transform to martensite upon water or air cooling after austempering. The presence of hardenability alloying elements in the alloy composition may as well play some role in enhancing the martensite formation.

For IADI, partially austenitized at 820 °C, the low austenitizing temperature will result in low C-austenite, which raises the M s temperature and decreases the hardenability; hence, higher amounts of martensite will form upon further cooling. The relatively low austempering temperature of IADI (300 °C) apparently plays a role in decreasing the C-diffusion rate and lowering the austenite stability, as the case with the alloy ADI-275. In both mechanisms, the low C-content of austenite decreases its stability and promotes more martensite formation. Figure 5 a–d illustrates how the cutting force depends on the depth of cut at different cutting speeds for the investigated ADI-grades. Some remarks concluded from the illustrated data are summarized in the following discussion: In the alloys ADI-275 and ADI-375, the lowest cutting force reached about 350 N at the lowest cutting depth 0.5 mm and the slowest cutting speed of 55 m/min (Figure 5 a). At the same cutting depth, increasing the cutting speed from 55 to 90 m/min leads to a notable decrease in the cutting force especially at depth of cut 1.0 mm and 1.5 mm. Further increase in the cutting speed to 140 and 180 m/min results in a progressive increase in the cutting force (see Figure 5 b, c). A different behavior could be noticed at 2.0 mm depth of cut; the cutting force reached its maximum value (~ 950 N) at the slowest speed of 55 m/min. By increasing the cutting speed to 90 m/min., the cutting force decreased to about (~ 800 N) and then increased again to the same value (~ 950 N) when the cutting speed increased to 140 m/min. At the highest cutting speed of 180 m/min, a significant drop in the cutting force to a value lower than (~ 850 N) is observed in both mentioned ADI alloys (ADI-275 and ADI-375). It should be mentioned that the maximum cutting force reached about 980 N at the slowest cutting speed of 55 m/min and cutting depth 1.5 mm (Figure 5 c).

The cutting force values of the IADI alloy (Figure 5 a–d) were significantly lower than those noticed for the other two alloys apparently due to the lower hardness and considerable amounts of pro-eutectoid ferrite in the structure of this alloy. The maximum cutting force reaches a value of ~ 850 N at 2.0 mm cutting depth and 140 m/min cutting speed. Increasing the cutting speed to 180 m/min, the cutting force drops to much lower value of ~ 650 N. The lowest cutting force was observed at the lowest cutting depth 0.5 mm and at the slowest cutting speed of 55 m/min. With increasing the cutting speed to 90 and 140 m/min, the recorded cutting force value seems to be constant (< 300 N). Then, it drops to a much lower value of ~ 200 N with the increase in the cutting speed to 180 m/min. To confirm the decisive role of strain hardening of ADI and the retained austenite transformation to martensite on the machinability behavior of ADI alloys, the martensite content in the microstructure of different ADI alloys after each turning operation with different cutting depths was determined by XRD. Figure 6 illustrates the variation in both martensite content and cutting force with the cutting depth of ADI-275 and ADI-375.

As previously shown in Figure 4 , the martensite contents of the ADI-275 and ADI-375 were 9.71% and 0.46%, respectively. Such wide variation was discussed before in 4.2. It is evident that the increase in cutting force is always associated with a corresponding increase in the martensite content when the cutting depth was increased from 0.5 to 2.0 mm at 55 and 90 m/min cutting speeds. It was noticed that in the ADI-375, although having only 0.46% martensite in the structure before machining, this ratio increases with increasing cutting depth to 2.0 mm to reach about ~ 23% martensite with a corresponding increase in the cutting force. On the other hand, the alloy ADI-275 started with about 9.71% martensite before machining. Obviously, all the retained austenite in the original structure (about ~ 11.28%) was subjected to martensitic transformation to reach a total level of martensite of ~ 21% at a cutting depth of 2.0 mm which is very close to the martensitic level reached by ADI-375 at the same depth of cut.
Finally, the two alloys being subjected to a cutting depth of 2.0 mm had the same total martensite (which is the sum of original content before machining plus the martensite formed by deformation-induced transformation from the retained austenite). The fact that the two alloys—ADI-375 and ADI-275—reached to the same cutting force at 2.0 mm depth of cut gives a good indication that the martensitic transformation due to induced strains is closely related to the machinability behavior of the ADI-alloys (Figure 7 a–d). Such correlation is even more evident with the ADI-375 alloy at 90 m/min cutting speed (see Figure 7 c). At 1.5 mm cutting depth, the martensitic content and the force of cutting reached almost the same levels observed for the other previously discussed cases of ADI-375 and ADI-275 at 55 and 90 m/min cutting speed (Figure 5 c). However, increasing the cutting depth to 2.0 mm, both the martensite content and the cutting force decreased in very similar manner. Obviously 2.0 mm depth of cut is deeper than the hardened layer, and so the cutting tool avoids that hard layer and penetrates deeper in the softer base metal.

ADI-275 at 90 m/min cutting speed shows a continuous increase in cutting force by increasing the depth of cut (see Figure 7 a–d). This may indicate that the hardened layer was thicker than 2.0 mm. Making significant use of the heat tinting etching process, the fluctuation of martensite content with the cutting depth was further validated (Figure 8 ). Figures 9 and 10 show the change of the measured flank wear (VB max ) of the CVD and CBN tools, respectively, with time for all investigated alloys at two different turning speeds. At a high turning speed of 400 m/min, the hardest ADI grade, ADI-275, showed the highest tool wear. Increasing the austempering temperature to 375 °C shows a progressive increase in the tool wear at a turning speed of 400 m/min and its value approaches that one of the wear levels of ADI-275-200 m/min, although this material is much softer than ADI-275. By decreasing the turning speed to 200 m/min, the tool life is almost doubled two times for both ADI-275 and ADI-375 alloys. The fact that the two alloys-ADI-275 and ADI-375 reached approx. the same wear level gives a good agreement with the discussion about the strain hardening behavior of these alloys. It should be noticed that the trending of the tool wear curves related to the alloys ADI-275 and ADI-375 is virtually the same, which suggests that the main tool wear mechanism is probably the same for the two alloys.

The tool wear during turning of the IADI alloy is much less than that of the other two ADI alloys described above at the two turning speeds, evidently as a result of the alloy’s higher proportion of pro-eutectoid ferrite and lower hardness. The tool wear curve of the IADI demonstrates a steady state zone (from 30 to 70 s) with a considerable low wear rate, demonstrating that the utilized cutting speed is suitable for this CVD tool at a turning speed of 200 m/min. The fact that CBN tools were developed with advanced mechanical properties, such as toughness and wear resistance, became suitable for tooling applications at severe conditions. It can be observed that the wear rate of the CBN is very low when compared with the wear rate of the CVD tools. A high initial increase in flank wear value on the CBN tool can be noticed which varies according to the material properties. After that, the wear rate is slowly increasing, showing an interesting result. The machining process for IADI alloy using the CBN tool shows the lowest wear rate among the other ADI alloys by reaching a value of VB max (~ 0,07–0,15 mm) with time (>100 s) at the two different cutting speeds.
Figure 11 shows the surface roughness results obtained from the machining tests of the three investigated ADI alloys. The surface roughness values are ranging between R a = 0.5 and 3.0 µm. There are different interlinked factors that control the final surface quality of the developed ADI alloys, cutting parameters such as cutting speed and depth of cut and the microstructural constituents of each grade. Generally speaking, as cutting speed increased, the surface roughness is decreased, i.e., achieving better quality surface. This effect is attributed to the built-up edge (BUE) formation at the tool tip. Cutting at low speed increases the adherence tendency between the tool and workpiece leading to increased BUE formation and deterioration of the surface quality. Moreover, a shallower depth of cut always improves the machinability. The final surface quality of each grade is greatly influenced by the morphology and amount of ferrite. From Figure 11 , a higher ferrite content in the matrix leads to deteriorating the surface quality of the investigated alloys. This could explain the highest surface roughness values in all machining experiments obtained for IADI grades, which mainly contain the highest ferrite content. ADI-275 showed lower surface roughness than ADI-375; this is because the microstructure of ADI-275 contains very fine ausferrite unlike ADI-375 which contains thick ausferrite lathes.

An interesting behavior could be observed; at a cutting depth of cut 1.0 mm, the surface roughness is increasing in both ADI-275 and ADI-375 with increasing cutting speed. However, at depth of 2.0 mm, as the cutting speed is increased, the surface roughness is decreasing in both ADI-275 and ADI-375. The combined effect of cutting speed at higher values with deeper depth of cut could result in increasing the thermal softening effect and giving a better machined surface, while higher values of cutting speed with shallower depth of cut lead to the strain hardening effect and the material becomes more difficult to machine with inferior surface quality. The machinability of ADI alloys can also be evaluated using the chip formation criterion. Figures 12 and 13 display the chips produced when the three ADI materials were machined at two different cutting speeds, varied cut depths at the same feed rate. According to reports, the workpiece material, cutting tool geometry, machining environment (such as wet or dry conditions), and machining parameters (such as depth of cut, cutting speed, and feed rate) all have a significant impact on the final chip shape.

Chips that were segmented, flatten, and discontinuous were noticed when the three ADI grades were being turned. When the cutting speed was increased from 200 to 400 m/min, there were almost no difference that could be noticed in the chips. However, the tendency to produce thicker chips increases with increasing depth of cut. The machinability characteristics of three different austempered ductile irons, namely ADI-375, ADI-275, and IADI, were evaluated using three machinability indicators: cutting force, tool wear, and surface roughness. The machinability results indicated that the increase in cutting force is always associated with a corresponding increase in the martensite content with increasing cutting depth from 0.5 to 2.0 mm. Ferrite content and morphology have a great impact on the overall surface finish of each grade as it leads to deteriorating the surface characteristics of the investigated alloys. This could explain the highest roughness values across all processing experiments obtained in IADI grade, which mainly contain the highest ferrite contents.


Cycle no. | ADI Grade | Austenitizing temperature-time | Austempering temperature-time |
|---|---|---|---|
1 | ADI-275 | 900 °C–90 min | 275 °C–90 min |
2 | ADI-375 | 900 °C–90 min | 375 °C–90 min |
3 | IADI | 820 °C–90 min | 325 °C–90 min |
Run no | Depth of cut, ac, mm | Cutting speed,VC, m/min | Feed rate,f,mm/rev |
|---|---|---|---|
1 | 0.5 | 55 | 0.214 |
2 | 90 | ||
3 | 140 | ||
4 | 180 | ||
5 | 1.0 | 55 | |
6 | 90 | ||
7 | 140 | ||
8 | 180 | ||
9 | 1.5 | 55 | |
10 | 90 | ||
11 | 140 | ||
12 | 180 | ||
13 | 2.0 | 55 | |
14 | 90 | ||
15 | 140 | ||
16 | 180 |
Samples | F, % | P, % | γ, % | M, % | N.C, N.mm-2 | SP, % | Hardness, HB30 |
|---|---|---|---|---|---|---|---|
As cast | 21.7 | 68.4 | – | – | 172 | 81.86 | 195 |
ADI-275 | 79.03 ± 4.3 | – | 11.26 ± 0.85 | 9.71 ± 0.77 | – | – | 469 |
ADI-375 | 64.04 ± 5.66 | – | 35.50 ± 3.62 | 0.46 ± 0.52 | – | – | 322 |
IADI | 84.81 ± 0.12 | – | 4.95 ± 0.24 | 10.24 ± 4.64 | – | – | 255 |
Hussein, Mona, Ahmed, Mostafa, Soliman, Mohamed, Mohamed, Lamiaa Z., Palkowski, Heinz, Rashad, Ragaie M., Nofal, A.. Influence of Austenite Stability on the Machinability of Different Grades of Austempered Ductile Iron (ADI) During Dry Turning Machining. DOI: 10.1007/s40962-023-01063-0. CC BY 4.0。 Original paper · PDF · CC BY 4.0 ·