Cast Zinc-Aluminum-Magnesium Alloy: Magnesium Content and Corrosion Resistance


Published: 

2023-01-20

The relationship between microstructure refinement, corrosion products, and corrosion resistance was investigated in Zn-0.5Al alloys with varying magnesium contents, using microstructural analysis, polarization measurements, and impedance spectroscopy.

Figure 1 . Position of specimens for microstructure investigation and corrosion tests. 44

Figure 1 . Position of specimens for microstructure investigation and corrosion tests. 44

Alloy Preparation and Electrochemical Testing

Zn–Al–Mg alloys combine useful casting characteristics with opportunities for microstructural control. This study uses previously prepared Zn–0.5Al–Mg alloys to compare microstructures and electrochemical responses at different Mg contents in simulated body fluid. Its objective is to identify compositions with degradation rates of interest for orthopedic implant research; the experiments concern in-vitro corrosion and the associated microstructural mechanisms.

Zn–0.5wt%Al–Mg alloys with Mg additives of (0.0, 0.2, 0.4, 0.6, 0.8 and 1.0 wt%) were received from the previous report. These samples were prepared by melting pure Zn (99.99 %), Al (99.99 %) and commercial pure Mg (99.96 %) ingots. An electric resistance furnace was employed, and the temperature reached 690 °C ± 5 °C. The mixture was then stirred lightly with a graphite rod to ensure good mixing. After skimming the slag, the molten alloys were then poured into a preheated cylindrical cast iron mold (150 °C) of dimensions of 100 mm outer diameter, 40 mm inner diameter and 250 mm height. The specimens were prepared as discs of 6 mm in diameter and 2 mm in thickness. Each disc was held by stainless steel rod sheathed with teflon for complete isolation when immersed in the electrolyte solution. The discs were fine polished using SiC papers up to 2400 grit and then cleaned ultrasonically in deionized water for 5 minutes. Afterwards, the specimens were etched in a 3 wt% Nital solution for 5 minutes at room temperature then rinsed with water and ethanol followed by washing with anhydrous ethyl alcohol and drying. The chemical analysis of the investigated alloys was determined with X-ray fluorescence analyzer (XRF) (model Axios advanced-PANA- LYTCAL, Netherlands) and presented in Table 1 .

A scanning electron microscopy (JEOL- JSM-5410, Japan) equipped with an energy dispersive spectrometer unit (EDS-Oxford) was used to study the surface morphologies of alloys and chemical composition, respectively. X-ray diffractometer (Bruker AXS-D8, Advance, Germany, operated at 35 KV and 45 mA with CuKα radiation λ = 0.1540 nm) was performed to find out the structure of different phases. Specimens were taken at the positions illustrated in Figure 1. The position of specimens for microstructure and corrosion investigations were shown in Figure 1 . Electrochemical measurements using (potentiostat/galvanostat, Autolab PGSTAT 302N, Netherlands equipped with the NOVA software package) were performed at 37 ºC in SBF solution (pH 7.4) containing (g/l (NaCl :8, CaCl 2 : 0.14, KCl :0.4, NaHCO 3 : 0.35, C 6 H 12 O 6 : 1, NaH 2 PO 4 : 0.1, MgCl 2 . 6H 2 O :0.1, Na 2 HPO 4 .2H 2 O : 0.06 and MgSO 4 .7H 2 O: 0.06.at pH 7.4. A conventional three-electrode system in which Ag/AgCl was utilized as the reference electrode, while a platinum as a counter electrode and tested alloys were used as the working electrodes. The circular area that was exposed to the electrolyte solution was 0.785 cm 2 . Stabilization time of 30 min at the open circuit potentials (OCP) was recorded before starting the potentiodynamic measurements. Electrochemical impedance spectroscopy (EIS) was completed in a frequency range of 10 mHz 100 kHz with a perturbation amplitude of 5 mV. Potentiodynamic polarization curves were performed from -1.4 mV to -0.2 mV at a scan rate of 1 mV/s. For reproducibly purposes, two tests were applied for each sample.

tissue change and corrosion mechanism

Figure 2 showed the optical microstructures of the investigated Zn-0.5Al-Mg alloys with and without Mg additions. It was obvious that without Mg additions, the microstructure of the Zn-0.5Al based alloy consisted of Zn dendrites with an average size of 164 μm and a Zn-Al eutectic phase. However, the microstructure of the alloys containing Mg, as shown in Figure 2 consisted of primary Zn dendrites surrounded by binary (Zn + Mg_2Zn_11 ) or (Zn + MgZn_2 ) and ternary (Zn + Mg_2Zn_11 + Al) eutectic phases. With increased concentrations of Mg, the degree of fineness of Zn dendrites increased and their size decreased from 165 to 110 μm with 0.2 wt% Mg and further down to 40 μm with 0.8 wt% Mg and their morphologies changed gradually to nearly polygonal shapes with 0.8 wt% Mg addition (Figure 2 e). This grain refinement effect can be attributed to the growth restriction factor of Mg which restricted the growth of Zn dendrites. With further Mg additions up to (1 wt%), the microstructure of Zn became coarse dendrites (Figure 2 f) and their size increased again. This result is in agreement with Krieg et al. who concluded in their work that the magnesium content had a great influence on the microstructure of the alloy where the degree of fineness of the microstructure increased with increasing magnesium contents.

Figure 2 . Optical micrographs of the as-cast Zn–0.5Al–Mg alloys 44 (a) 0 (b) 0.2 (c) 0.4 (d) 0.6 (e) 0.8 (f) 1 wt% Mg concentrations.
Figure 2 . Optical micrographs of the as-cast Zn–0.5Al–Mg alloys 44 (a) 0 (b) 0.2 (c) 0.4 (d) 0.6 (e) 0.8 (f) 1 wt% Mg concentrations.

The XRD patterns of ternary Zn–Al–Mg alloys were shown in Figure 3 and are compared with those of binary Zn–Al alloy. The results are consistent with the microstructure shown in Figure 2 . In the Zn–Al alloy, intermetallic compounds containing Zn–Al were not identified, it was made up of main Zn phases due to the high solubility of Al in Zn matrix. In the XRD graph of as-cast Zn–Al–Mg alloy, there were no Zn–Al–Mg ternary intermetallic compounds recognized. Two phases were mainly indexed: the Zn matrix and second intermetallic phases. In the Zn–Al–0.2 Mg, A peak appeared indicating traces of Orthorhombic Mg_7Zn_3 intermetallic compounds. However, on the addition of 0.6 Mg, peaks of Al and highly crystalline hexagonal MgZn_2 phases were identified while highly crystalline cubic lattice Mg_2Zn_11 phases were detected in the Zn–Al–1.0 Mg. To study the influence of Mg content on the corrosion process of Zn-Al alloys, potentiodynamic polarization was utilized on the as Zn alloys in SBF solution at pH 7.4 and temperature 37 ºC. The Tafel extrapolation method was used to extract the corrosion current density i_Corr and the corrosion potential E_corr data from linear sections of polarization curves. Through this procedure, the linear part of the anodic and cathodic branches is extended, and their collision points indicate the i_Corr and E_corr coordinates and the slope of each branch shows the Tafel slopes. Higher values of E_corr suggest that the samples have better corrosion resistance, while elevated values of i_Corr indicates that the samples are suffering from fast corrosion or degradation rates. Polarization curves of the as-prepared Zn–0.5Al–Mg alloys in simulated body fluid were performed and compared to Zn–Al alloy in Figure 4 .

Figure 3 . XRD Results of the investigated Zn alloys.
Figure 3 . XRD Results of the investigated Zn alloys.
Figure 4 . Potentiodynamic polarization curves of as cast prepared alloys in SBF.
Figure 4 . Potentiodynamic polarization curves of as cast prepared alloys in SBF.

It can be noticed from the polarization curves in Figure 4 , that the corrosion potential E_corr of all alloys shifted to the more positive direction as compared to the Zn-Al alloy associated with higher corrosion current densities i_corr except Zn–Al–0.6Mg which had a more promising value of i_corr of 22 μ A/cm^2 and a slight negative shift in the corrosion potential E_corr reaching a value of −0.946 V. The negative shift of the corrosion potential of the Zn–Al–0.6Mg alloy can be attributed to a rise in the anodic reactions due to the formation of oxide protective films on the surface of the alloy at the initial stages of corrosion. The corrosion behavior of Zn–Al–Mg alloys in simulated body fluid is proposed in the following reactions which mainly consist of the following anodic and cathodic reactions:

2Zn→2Zn2++4e−(1)
2H2O+O2+4e−→4OH−(2)
Zn2++2OH−→Zn(OH)2(3)

However, the main corrosion product precipitated on the surface is solid Zn( OH )_2 which protects the Zn alloy from further corrosion. Such protection effect is relatively weak since the Zn( OH )_2 layer is not compact. Simulated Body fluid (SBF) which is a corrosive medium containing aggressive chloride ions with small radius, easily penetrates the loose Zn( OH )_2 layer, forming soluble zinc chloride according to Eqn. ( 4 ). Therefore, the corrosion protection of Zn surfaces by Zn( OH )_2 is not efficient in presence of Cl − ions.

Zn(OH)2+2Cl−→Zn2++2Cl−+2OH−(4)

The released Zn ions can further react with phosphate ions to form insoluble Zn phosphate (or hepatite):

Zn2++2HPO42−+2OH−+2H2O→Zn3(PO4)2·4(H2O)(5)

This insoluble compound tends to nucleate and form on the surface of the specimens decreasing the corrosion reactions. The deposition of biocompatible zinc phosphate on zinc substrate simulates new bone formation in human body and thereby accelerates the healing of bone tissue. Moreover, the production of magnesium hydroxyl carbonates was mentioned for Zn–Mg alloys:

2Mg2++2OH−+CO2−→Mg2(OH)2CO3(6)

It was proposed that Mg can enhance the corrosion resistance of Zn-based alloys by the formation of electrochemically inert compounds such as Mg 2 (OH) 2 CO 3 on the surface of investigated samples. Also, Mg-containing a form of simonkolleite has been reported to act as a corrosion inhibitor. The polarization resistance and the corrosion current densities are identified through Tafel slopes by Stern–Geary Eqn: ,

Rp=βaβc2.3ICorr(βa+βc)(7)

Where ( β a and β c ) are the anodic and cathodic Tafel slopes. The corrosion current density ( i_Corr ) is related to the corrosion rate ( R_i ) by the following Eqn. ( 8 )

Ri=KicorrEWd(8)

Where: R_i is given in mm/year, i_Corr in µA/cm 2 , K = 3.27 × 10^ - 3 mm g/μ A cm year , EW is the equivalent weight and d is the density of the base zinc metal which is 7.13 g/cm^3 . The corrosion parameters derived from the polarization curves such as, corrosion potential ( E_Corr ), corrosion current density ( I_Corr ), polarization resistance ( R p ) and corrosion rate ( R i ) were recorded in Table 2 . The results in Table 2 revealed that the Zn–0.5Al and Zn–0.5Al-0.6Mg alloy exhibited good corrosion resistance as they were close to the suitable corrosion rates for orthopedic biodegradable materials. On the addition of 0.2-0.4 wt% Mg, the corrosion inhibition of the ternary alloys decreased suggesting surface reactivity and unstable corrosion products leading to increased corrosion attacks. However, the addition of 0.6 wt% Mg to the alloy exhibited a favorable corrosion resistance which can be ascribed to the formation of fine MgZn 2 intermetallic phases distributed in the eutectic Zn matrix with the inclusion of higher amounts of Mg as confirmed by the XRD in Figure 3 . These secondary phases are homogenously dispersed in the matrix, leading to the generation of a uniform surface film of Mg-containing corrosion products which act as a corrosion boundary that can hinder the occurrence of localized corrosion and can effectively protect the Zn-based alloy. Also, the high corrosion resistance of the alloy could be related to the uniform distribution of Al phases in the microstructure which can hinder the chance of corrosion attack on the passive film.

However, higher Mg concentrations up to 1% wt led to the increase in the corrosion rates of the Zn–Al–Mg alloy which can be as a result of formation of galvanic micro-cells between Zn and Mg 2 Zn 11 , therefore increasing the degradation rate of the base alloy. This result is in agreement with the XRD (Figure 3 ) where cubic lattice Mg 2 Zn 11 phases were detected in Zn–Al–1.0 Mg. This suggestion was also proposed by Mostaed et al. , who mentioned that galvanic corrosion due to Mg 2 Zn 11 enhanced the corrosion rates in Zn- x Mg alloys. Moreover, the decrease in corrosion resistance with higher Mg content up to 1.0 Mg are in good agreement with a previous study. It was clear from Table 2 that the Zn-0.5Al-0.6Mg ternary alloy had the lowest degradation rate of 0.33 mm/year as compared to the other investigated alloys which satisfies the requirements for ideal corrosion rates in orthopedic implants of less than 0.5 mm/year. This corrosion rate helps the implantable metal alloy to survive in the body during the healing process of the bone tissue. This finding is close to another work by Bakhsheshi-Rad et al. who studied the corrosion behavior and biocompatibility of Zn–0.5Al and ternary Zn–0.5Al–xMg biodegradable alloys by altering Mg contents. They concluded that the Zn–0.5Al–0.5Mg alloy exhibited the lowest corrosion degradation rates and attained suitable biocompatibility and mechanical properties as a biodegradable implantable material.

Figure 5 shows the Nyquist plots of the Zn–0.5Al–Mg alloys with different Mg contents using electrochemical impedance spectroscopy (EIS) technique in SBF solution at pH 7.4 and temperature 37 ºC. The impedance study confirms the previously obtained results by polarization. The obtained Nyquist plots consisted of one capacitive semicircle loop with different diameters; an increase in the size of the semicircle indicates an increase of corrosion resistance. It was observed that that the best corrosion performance was for the Zn–Al–0.6Mg since it attained the largest loop diameter. In order to enable an accurate analysis of the impedance diagrams, the equivalent circuit model was shown in Figure 6 . The most fitted electric model to explain the corrosion process is the simple model one-time constant. The equivalent circuit consisted of a constant phase element (CPE) which is parallel to a polarization resistance (charge transfer resistance) of the coating surface R p , both are in series with solution resistance Rs. Constant phase element (CPE) included in this circuit compensates the action of capacitor owing to surface heterogeneity and is defined by impedance value which can be characterized by the following equation:

Figure 5 . Nyquist plots for as cast prepared alloys in SBF.
Figure 5 . Nyquist plots for as cast prepared alloys in SBF.
Figure 6 . Equivalent circuits used for modeling of experimental EIS data.
Figure 6 . Equivalent circuits used for modeling of experimental EIS data.
ZCPE=[C(jω)α]−1(9)

Here α is the surface heterogeneity exponent, 0≤α≤1; j is the imaginary unit (j²=−1), and ω=2πf is the angular frequency in rad/s, with f in Hz. Table 3 reports the EIS results. Zn–Al–0.6Mg has Rp=0.35 kΩ·cm², higher than the other alloys. Rp characterizes resistance to charge transfer but does not alone establish all protective properties of the corrosion film. Combined polarization, impedance and microstructural evidence indicates that the 0.6 wt% Mg alloy has favorable corrosion behavior within the tested set.

SEM images (low-and high-resolution images) and EDS spectra analysis of the most corroded regions of the surfaces of the investigated Zn ternary alloys after electrochemical tests in SBF were shown in Figures 7 and 8 . It was apparent that the surface of the Zn–0.5 Al alloy (Figure 6 i) was covered with pores and a few number of large corroded pits due to the breakage of oxide films by attacking of chloride ions and phosphate ions in SBF solution. However, the corroded areas were increased with the addition of 0.2 wt% Mg (Figure. 7 ii) On the addition of 0.6 wt% Mg, it was clear from Figure ( 7 iii) that the corroded areas apparently decreased since many areas of the base alloy were not attacked by corrosion. Furthermore, the Zn-0.5Al-1Mg alloy (Figure. 7 iv) showed increased areas of anodic attacks on the surface. The EDS results of different regions on the surfaces of the Zn alloys were listed in Table 4 for purpose of comparison. The results revealed that besides the basic components of the alloys, one can observe that the corrosion products included Phosphorus, Chloride and Calcium originating from the simulated body fluid. Hence, it can be proposed that the surfaces of the corroded zinc alloys were dominated by aluminum oxide/hydroxide, insoluble calcium–Zinc phosphates, zinc hydroxide, zinc carbonates, insoluble calcium–magnesium phosphates or magnesium hydroxyl carbonates as shown from the previous corrosion reactions. These corrosion products were reported to be protective passive layers that protects the Zn-based alloys from further attack from the simulated body fluid (SBF).

Figure 7 . SEM (100 µm and 200 µm magnification) of corroded surfaces after immersion of the investigated samples in SBF (i) Zn0.5Al , (ii) Zn0.5Al0.2Mg, (iii) Zn0.5Al0.6Mg, (iv) Zn0.5Al1Mg.
Figure 7 . SEM (100 µm and 200 µm magnification) of corroded surfaces after immersion of the investigated samples in SBF (i) Zn0.5Al , (ii) Zn0.5Al0.2Mg, (iii) Zn0.5Al0.6Mg, (iv) Zn0.5Al1Mg.

It was also noticed from Table 4 that the main differences between corroded areas (A, C, E and G) and flat areas (B, D, F and H) are in the concentrations (wt%) of oxygen and aluminum where these concentrations greatly increased in the corroded regions which can be attributed to the formation of Aluminum oxides. However, there were not many differences between the concentrations of P, Cl or Ca. The corrosion products also included Mg phases so magnesium corrosion products like magnesium hydroxyl carbonates or phosphates might have been produced. Hence, it was concluded in this work that the inclusion of 0.6 wt% Mg to the Zn based alloy helped in the increase of fineness of the microstructure of the alloy. According to the previous study, the authors concluded that Mg helped in the homogeneous distribution of Al phases in the Zn matrix which helped in the development of Aluminum oxide protective layers. It is also known that Al is less noble than zinc, therefore it is expected to be preferentially oxidized than Zn and hence protecting Zn from further corrosion. This was confirmed in this work since the EDS analysis of the corroded regions of the samples showed increased concentrations of Al and oxygen in the corroded areas revealing the formation of Aluminum oxide films. Volovitch et al. reported that aluminum formed basic aluminum-oxides in the initial stages of corrosion of a Zn-Al-Mg alloy

The fine microstructure of the Zn–0.5Al–0.6Mg alloy also helped to increase its corrosion resistance. This result is close to a work performed by Yao et al. who analyzed Zn-Mg alloys with different Mg concentrations and noticed that an alloy containing 3wt% Mg was more resistant to corrosion due to the nanostructure of the alloy. However, when 1 wt% Mg was added, it affected negatively on the corrosion rates due to the coarse structure of the alloy and the increase in grain size which contributes to the inhomogeneous distribution of corrosion products on the alloy surface and consequently less corrosion resistance. Moreover, the formation of MgZn_2 and Mg_2 Zn_11 intermetallic phases seem to have an important role in the corrosion resistance of the alloys. Owing to the higher standard electrode potential of Mg element than Zn, intermetallic phases (eutectic structures) are more vulnerable to be eroded than Zn matrix while the Zn cathode is protected. MgZn_2 intermetallic phases were formed in the Zn–0.5Al–0.6Mg alloy as shown from the XRD (Figure 3 ). The propagation of corrosion areas extending along the grain boundaries of eutectic structures was seen in Figure ( 7 )iii) which might be attributed to the fine structure and homogeneous distribution of intermetallic phases in the Zn matrix and along the grain boundaries. This might have helped in the production of Mg-based oxide films along with other corrosion products preventing the Zn alloy from further exposition to the electrolyte.

Prosek et al. confirmed that the superior corrosion properties of Zn-Mg alloys are related to the presences of MgZn_2 and Mg_2Zn_11 intermetallic (IMC) phases. However, further additions of Mg above 0.6 wt % led to the increase in the percentage of Mg_2Zn_11 secondary intermetallic phases which caused accelerated galvanic corrosion between Zn and the precipitated secondary phases and consequently deteriorated the corrosion inhibition effect of Mg and reduced the corrosion resistance of the alloy. In this study, several Zn–0.5Al–Mg cast alloys were received to study the influence of Mg concentrations on the microstructure and corrosion behavior of the Zn-based alloys. It was the aim of this work to determine the best composition of the Zn ternary alloy to be employed in orthopedic biodegradable implant applications. The SEM analysis revealed that Magnesium had a great effect on the microstructure of the alloy where the degree of fineness of the microstructure increased with increasing magnesium contents up to 0.6 wt%. However further additions of Mg led to the formation of coarse microstructures. The X-ray diffraction confirmed the production of MgZn_2 and Mg_2 Zn_11 secondary phases.

Moreover, polarization analyses revealed that the ZnAl0.6Mg ternary alloy had the lowest degradation rate of 0.33 mm/year as compared to the other investigated alloys which satisfies the requirements for ideal corrosion rates in orthopedic implants of less than 0.5 mm/year. This corrosion rate helps the implantable metal alloy to last in the body until healing of the bone tissue. The superior corrosion properties of Zn-Al-0.6Mg alloy was contributed to the fine structure, uniform distribution of Aluminum oxide passive layers and the uniform formation of MgZn 2 phase precipitated in the Zn-rich matrix and along the grain boundaries which provided the best corrosion stability in SBF.

Figure 8 . EDS Spectra analysis of the investigated Zn based alloys, (a) Zn-0.5Al, (b) Zn-0.5Al-0.2Mg,(c) Zn-0.5Al-0.6Mg, (d) Zn-0.5Al-1Mg.
Figure 8 . EDS Spectra analysis of the investigated Zn based alloys, (a) Zn-0.5Al, (b) Zn-0.5Al-0.2Mg,(c) Zn-0.5Al-0.6Mg, (d) Zn-0.5Al-1Mg.
Table 1. The Chemical Analysis of the Investigated Alloys (wt%)

Investigated alloys

Zn

Al

Mg

 

ZnAl

Bal.

0.45

–

 

ZnAl + 0.2Mg

Bal.

0.45

0.17

 

ZnAl + 0.4Mg

Bal.

0.45

0.36

 

ZnAl + 0.6Mg

Bal.

0.44

0.56

 

ZnAl + 0.8Mg

Bal.

0.46

0.75

 

ZnAl + 1Mg

Bal.

0.43

0.96

 
Table 2. Electrochemical Parameters and Corrosion Rates Obtained by Polarization Tests

Samples

Ecorr(V)

iCorr(μAcm2)

Rp(KΩ)

Ri(mmy)

Zn–0.5Al

−0.920

36

0.50

0.54

Zn–0.5Al–0.2Mg

−0.900

52

0.83

0.79

Zn–0.5Al–0.4Mg

−0.914

63

0.81

0.95

Zn–0.5Al–0.6M g

−0.946

22

1.11

0.33

Zn–0.5Al–0.8M g

−0.902

42

0.77

0.63

Zn–0.5Al–1.0Mg

−0.892

50

0.86

0.75

Table 3. Electrochemical Impedance Parameters

Sample

Rp (kΩcm2)

CPE(μFcm−2)

α

Rs(Ωcm2)

Zn–Al

0.26

34

0.92

10

Zn–Al–0.2Mg

0.23

44

0.78

16

Zn–Al–0.4 Mg

0.22

68

0.82

28

Zn–Al–0.6Mg

0.35

22

0.76

21

Zn–Al–0.8Mg

0.24

40

0.84

18

Zn–Al–1.0Mg

0.22

46

0.79

20

Hammam, Rania E., Abdel-Gawad, Soha A., Moussa, Mohamed E., Shoeib, Madiha, El-Hadad, Shimaa. Study of Microstructure and Corrosion Behavior of Cast Zn–Al–Mg Alloys. DOI: 10.1007/s40962-022-00944-0. CC BY 4.0。 Original paper · PDF · CC BY 4.0 ·