Aluminum-Copper Composite Casting: Oxygen-Free Interface and Thermal Conductivity


Published: 

2022-12-15

Aluminum–copper composite casting was performed in a silane‑containing inert atmosphere, and the effects of crucible and mold temperatures on the microstructure, thickness, and thermal conductivity of the bonding zone were investigated.

Figure 1 . (a) Top view showing locations of the ∅ 8 mm and ∅ 10 mm specimens; (b) corresponding side-view with target layer thicknesses after machining.

Figure 1 . (a) Top view showing locations of the ∅ 8 mm and ∅ 10 mm specimens; (b) corresponding side-view with target layer thicknesses after machining.

Anaerobic Atmosphere, Casting, and Characterization Methods

In this study, a novel approach was developed to prevent the formation of oxide layers on the materials prior to casting that occur in an inert gas atmosphere. Since even high-purity inert gases such as argon 5.0 (99.999% purity) still contain approximately 0.05 ppmv oxygen, their use cannot prevent the immediate re-formation of an oxygen monolayer on a deoxidized metal surface. In contrast, the approach employed in the present study aims at eliminating the formation of oxide layers on both the copper inserts as well as on the aluminum melt by reducing the oxygen activity to extremely low levels. This way, collisions of oxygen molecules with the deoxidized surface can be avoided at least for the duration of the actual casting process. As calculated by Holländer et al., a thermodynamic oxygen activity as low as < 10 −32 at 800 °C could potentially be achieved under ideal conditions, such as those that exist in an extreme high vacuum. Due to the challenges of generating an extremely high vacuum, the approach pursued here is to create an XHV-adequate atmosphere by doping high-purity argon (99.999% Ar) with small amounts of SiH 4 (monosilane). In the inert gas atmosphere, the silane reacts with the residual oxygen and water to form non-reactive silane dioxide, thus removing both educts from the environment:

SiH4(g)+2O2(g)→SiO2(s)+2H2O (g)(1)
SiH4(g)+2H2O (g)→ SiO2(s)+4H2(g)(2)

Cylindrical copper inserts with the dimensions Ø 31.8 mm × 2 mm were cut from a cold rolled oxygen free (OF) copper plate (Hans-Erich Gemmel & Co. GmbH, Berlin, Germany) by wire electrical discharge machining (EDM). The copper inserts featured a purity level of > 99.65% and were cleaned with ethanol prior to the compound casting experiments. The cast aluminum provided by Hydro Aluminium High Purity GmbH (Grevenbroich, Germany) had a purity of > 99.87%. Table 1 shows the chemical compositions of the metals used in this study as measured with a spark spectrometer. The aluminum ingots were heated to 200 °C to remove water residues and then cut into small pieces weighing 30–40 g. Subsequently, both the copper insert and the aluminum pieces were transferred into a glovebox with an XHV-adequate atmosphere via an airlock. Inside the glove box, the native oxide layer of the copper inlay was mechanically removed by grinding, using first 500 grit and then 1200 grit abrasive papers.

Compound casting was conducted in a glovebox (Labmaster 130, Mbraun GmbH, Munich, Germany), that was previously flooded with argon 4.8 (99.998% purity) to displace the air inside the entire box. To remove any residual oxygen and water, a prefabricated mixture of 99 mol-% argon 5.0 (99.999% purity) and 1 mol-% monosilane provided by Messer Industriegase GmbH (Bad Soden am Taunus, Germany) was infused. This procedure allowed for an inert gas atmosphere with an extremely low oxygen activity (reduction to 2 · 10 −18 vol.-%) in the process zone. The actual oxygen activity was continuously monitored with a calibrated λ-probe to make sure that an oxygen-free, XHV-adequate atmosphere was reliably established. The aluminum-copper compounds were produced by gravity die-casting. For this purpose, a casting device featuring a manually operated tilting graphite crucible with a filling volume of 130 ml was employed. The crucible and the aluminum placed inside were heated by a resistance heater coil whose temperature was controlled by means of a type-K thermocouple. The mold for the copper inserts as well as the casting channel had previously been coated with boron nitride (Henze Boron Nitride Products AG, Lauben, Germany). The mold had a drilled hole for the copper insert and another one for a thermocouple (type-K). Additionally, the temperature on the copper surface was measured with a contact thermocouple (type-K) before pouring the liquid aluminum onto it. Furthermore, a tube allowing direct doping of monosilane into the mold was installed. This way, the copper insert can be immersed in excess monosilane during heating in the mold, thus preventing its possible re-oxidation caused by gases released from the mold.

The casting experiments were performed with various temperature regimes to determine the influence of both the crucible and mold temperatures on the microstructure in the bonding zone between copper and aluminum. The minimum temperatures required to establish a successful bond in an XHV-adequate atmosphere had been determined in preliminary tests. For the experiments described here, the crucible temperature was varied between 750, 775, and 800 °C and the mold temperature from 300 °C to 500 °C at intervals of 50 °C. These temperatures cover the ranges typically used for the crucible and the mold when aiming to create a bond between aluminum and copper. The crucible was filled with 115 g aluminum at room temperature and then heated to the target temperature with a heating rate of 45 °C/min. The mold was heated with a heating rate of 20 °C/min. Depending on the selected casting parameters, the heating of the mold was timed to achieve both the selected crucible and mold temperatures simultaneously. After the target mold temperature was reached and the aluminum casting material had melted completely, the deoxidized copper insert was placed in the mold. A subsequent holding time of 5 min allowed for reaching stationary conditions. Finally, the molten aluminum was poured into the casting mold directly onto the copper insert and the heating was deactivated.

After cooling to room temperature, the aluminum-copper compound castings were removed from the glovebox and prepared for analysis. The specimens with an outer diameter of 31.8 mm were shortened by turning until the copper part had a plane-parallel thickness of 1 mm ± 0.1 mm in order to allow comparisons of the effects of different casting regimes. Four samples with a diameter of 10 mm each and three samples with a diameter of 8 mm each were then cut from the compounds by wire EDM. Figure 1 a illustrates the sample extraction positions from the cast compounds. Each specimen was turned plane-parallel to a total thickness of 3 mm (Figure 1 b). The samples with Ø 8 mm were used for microstructural characterization by scanning electron microscopy (SEM) and X-ray diffraction (XRD) and those with Ø 10 mm for the thermal conductivity measurements. For microstructural investigations, cross sections of the samples were metallographically prepared and etched. Grinding was performed with emery paper with grit sizes of 220, 400/500, 1200, and 2500. Finally, the samples were polished with diamond suspensions with grit sizes of 6 μm and 3 μm. Etching was performed using a hydrofluoric acid (10%) for aluminum and a mixture of potassium disulfite (25% to < 30%) and sodium thiosulfate pentahydrate (1% to < 5%) for copper. Images of the polished and etched specimens were taken by a BX53M optical microscope (Olympus Europa SE & Co. KG, Hamburg, Germany) and a DM4000M optical microscope (Leica Microsystems GmbH, Wetzlar, Germany).

To investigate the chemical composition of the compound zone, the polished samples were examined with a Zeiss Supra VP 55 field-emitter scanning electron microscope (SEM). For recording images dominated by material contrast, a backscattered electron detector (BSD) was employed. The chemical compositions were determined by energy dispersive X-ray spectroscopy (EDS) using a detector (Bruker AXS GmbH, Karlsruhe, Germany) in the SEM. The thermal conductivity of the castings was measured indirectly by irradiating the bottom surface of the samples with a xenon flash measuring device (LFA 447 from Netzsch-Gerätebau GmbH, Selb, Germany). The resulting temperature change of the upper surface of the sample was recorded with an indium antimonide infrared detector, which was cooled with liquid nitrogen. Prior to the measurements, the samples were coated with graphite on both sides to improve the absorption of the energy and the emission of infrared radiation to the detector. The thermal diffusivity was calculated using the pulse correction according to Cowan. The radiation losses as well as the convection on the surface were considered for the calculation.

Based on the measured thermal diffusivity a , the thermal conductivity λ can be calculated as :

λ=a·cp·ρ(3)

Where, c_p is the specific heat capacity and ρ is the density of the measured material.

λcompound zone=dcompoundzoneR(4)

In order to better assess the influence of the compound zone on the thermal conductivity between the copper insert and the aluminum casting material, the combined thermal conductivity was also determined. The thermal resistances of the compound zone ( R compoundzone ) and the aluminum casting material ( R Al ) were combined as

λcompound zone+Al=dcompound zone+dAlRcompound zone+RAl(5)

The combined thermal conductivity can potentially reach the thermal conductivity of the cast material, so ideally, the thermal resistance of the compound zone tends to zero. To shed light on the influence of different casting parameters (i.e., mold temperature and crucible temperature) on the thermal resistance of the compound zone, at least three samples of each parameter combination were measured to calculate average thermal conductivity values. Since thermal conductivity depends on the actual temperature, thermal diffusivity was measured in the temperature range between 25 °C and 200 °C, corresponding to the typical operating temperature range of heat exchangers. Higher temperatures could lead to increased diffusion processes, which would permanently affect the local microstructure of the compound zone.

Combining the regional organization and heat conduction results

The temperatures of the aluminum melt and the solid copper insert were monitored during the casting experiments. The process parameters resulting in formation of a metallurgical bond are provided in Table 2 . The temperature of the crucible (Figure 3 a) heated by means of a resistance coil was approx. 57 °C higher than the temperature of the aluminum melt for all castings. Figure 3 b shows that the mold temperature was also higher than the copper insert temperature. On average, the mold temperature exceeded the copper insert temperature by approx. 70 °C. This suggests that the process limit shown for the crucible as well as the mold temperatures in Table 2 is even lower if the actual contact temperatures between the bond partners are considered. Figure 4 shows light microscopic images of representative aluminum-copper compounds produced using different casting parameters. While copper can be recognized by its reddish colors, the cast aluminum appears in different shades of gray. In both samples, a distinct compound zone was formed, divided into different layers. With increasing casting temperatures, the overall thickness of the compound zone also increased. For the specimen cast at a crucible temperature of 800 °C and a mold temperature of 450 °C (Figure 4 a, a maximum layer thickness of ≈ 1.3 mm was observed. Lower temperatures led to a reduction of layer thicknesses, as shown exemplarily in Figure 4 b with a specimen cast featuring a crucible temperature of 750 °C and a mold temperature of 400 °C. Here, a layer thickness of ≈ 0.7 mm was obtained.

Figure 3 . Comparison of the nominal casting temperatures and the measured temperatures of aluminum (a) and copper (b).
Figure 3 . Comparison of the nominal casting temperatures and the measured temperatures of aluminum (a) and copper (b).
Figure 4 . Representative light microscopic images of etched specimens: (a) T crucible = 800 °C, T mold = 450 °C and (b) T crucible = 750 °C, T mold = 400 °C.
Figure 4 . Representative light microscopic images of etched specimens: (a) T crucible = 800 °C, T mold = 450 °C and (b) T crucible = 750 °C, T mold = 400 °C.

The dependence of the built thickness of the composite zone on the given temperatures of the crucible and the mold is illustrated in Figure 5 . It is evident that the temperature of the mold, and thus the one of the copper insert, had a greater influence on the total thickness of the compound zone than the temperature of the aluminum melt. For this reason, employing different crucible temperatures while keeping the mold temperature constant resulted in only slightly differing the thicknesses of the compound zones. Similarly, a tendency towards a higher overall thickness of the compound zone was also observed for increasing mold temperatures combined with a constant crucible temperature. By contrast, it was not possible to create a full bond at a low mold temperature of only 300 °C at a crucible temperature lower than 800 °C. Based on the aluminum-copper phase diagram, the chemical compositions obtained from the EDS provided initial indications of the phases present. The sample with the largest compound zone of ≈ 1.3 mm ( T crucible = 800 °C, T mold = 500 °C) is shown exemplarily in Figure 6 . The three differently shaped layers already detected by light microscopy were also evident in the SEM. In order to identify the different phases formed between copper and aluminum, EDS linescans were performed.

Figure 5 . Measured total thicknesses of the compound zones of samples cast at different temperature regimes.
Figure 5 . Measured total thicknesses of the compound zones of samples cast at different temperature regimes.
Figure 6 . (a) BSD overview image and corresponding (b) EDS linescan (trace is marked by arrow) with element concentration in at.-%, T crucible = 800 °C, T mold = 500 °C, (c) BSD image providing a detailed view of the 3rd layer and corresponding (d) EDS linescan with element concentration, (*) unidentified layer.
Figure 6 . (a) BSD overview image and corresponding (b) EDS linescan (trace is marked by arrow) with element concentration in at.-%, T crucible = 800 °C, T mold = 500 °C, (c) BSD image providing a detailed view of the 3rd layer and corresponding (d) EDS linescan with element concentration, (*) unidentified layer.

Given the aluminum base material, the first layer of the microstructure according to literature (e.g., Tavassoli et al., Greß et al. ) should be a eutectic structure consisting of a copper-rich aluminum solid solution (α-Al) and the θ-phase (Al 2 Cu). This is also the case with the compound castings created in XHV-adequate environment here: The BSD image (Figure 6 a) of the first layer reveals a thin lamellar microstructure characteristic of a eutectic microstructure. According to the EDS linescan (Figure 6 b), the eutectic microstructure consists of α-aluminum with a copper content of about 17 at.-% and the composition of the intermetallic fits the θ-phase (Al 2 Cu). In between the second layer – containing the θ-phase—and the copper substrate, another very narrow third layer was detected (Figure 6 c). This additional intermediate layer was also described by Tavassoli et al. In the EDS analysis, local element enrichment was detected. Specifically, the EDS analyses showed a chemical composition of about 35 at.-% aluminum and 65 at.-% copper for area "B" (Figure 6 d). In contrast to region "C", which featured irregular thickness, region "B" was more homogeneous across the whole sample. The corresponding diffraction patterns found in the XRD measurements were more distinct and the intermetallic γ-phase (Al 4 Cu 9 ) could be assigned to this region (PDF 00-024-0003 ). The third region “C” had a chemical composition of about 47 at.-% aluminum and 53 at.-% copper, indicating the presence of the η 2 (AlCu) phase. Between the regions B and C, another very thin and discontinuous layer, marked by (*) in Figure 6 c, could be detected in some of the BSD images. Its composition will have to be elucidated in a future investigation since the EDS analyses did not provide the necessary lateral resolution due to the excitation bulb.

To further substantiate the findings regarding the phase compositions, XRD analysis was performed on the prepared specimen. Diffractograms obtained at the different measuring points MP 1-5 are shown in Figure 7 . Employing the ICDD PDF2016 database, the diffraction patterns can be assigned to the θ-phase (Al 2 Cu) (PDF 01-076-3073) as well as to α-Al (PDF 03 065 2869). The incorporation of Cu atoms into the Al lattice causes a distortion resulting in a peak shift towards larger diffraction angles. The copper-containing aluminum thus featured a smaller unit cell than the base material. A decrease of the lattice constant along with increasing copper content was already demonstrated for copper-containing aluminum solid solutions. Consequently, the diffraction peaks at 2θ = 46° and 53.5° (Figure 7 ) can be assigned to the copper-rich aluminum solid solutions created by compound casting in XHV-adequate atmosphere. For measuring the thermal conductivity of the multilayer specimens, the outer layers (here: aluminum and copper) had to be fully characterized to calculate the contact resistance of the phase seam. Thermal conductivity λ was calculated using Eqn. ( 3 ). First, the averaged thermal diffusivities of three samples from each bulk material were measured. Since the standard deviations of the respective mean values were below 1 mm 2 /s for the thermal diffusivity and below 0.01 J/(g·K) for the specific heat capacity, the error bars in Figure 8 can barely be recognized. It was observed that the thermal diffusivity of copper first increases and then decreases with increasing temperature, whereas that of aluminum decreases continuously with increasing temperatures (Figure 8 ).

Figure 8 . Thermal conductivities of the bulk materials depending on ambient temperature.
Figure 8 . Thermal conductivities of the bulk materials depending on ambient temperature.

Thermal conductivities of the compound zones of the different specimens as well as the combined thermal conductivities were determined using Eqns. ( 4 ) and ( 5 ). Figure 9 shows the thermal conductivities calculated for the composite zones as a function of the mold temperature used. For the specimens produced at a nominal crucible temperature of 800 °C, lower mold temperatures were found to be resulting in higher thermal conductivities of the specimens. The range of thermal conductivities that could be achieved for the different aluminum-copper compounds produced are shown in Figure 10 . Depending on the casting parameters, different thicknesses of the compound zones were induced, which in turn resulted in a substantial change of the thermal conductivity. It needs to be noted that due to the usual local process fluctuations, it is not yet possible to produce compound zones featuring homogeneous thicknesses over the entire cross-section, which impairs the overall performance of the compound castings. Using Eqn. ( 5 ), the maximum possible combined thermal conductivity of an aluminum-copper compound is obtained for a contact resistance of zero, corresponding to the thermal conductivity of cast aluminum (234.7 W/(m·K)). Hence, in order to create the highest possible thermal conductivity, the total thickness of the compound zone should approach zero. Although the thermal conductivities demonstrated in Figure 10 are high, they still turn out to be substantially lower than the thermal conductivity of the cast pure aluminum. The highest thermal conductivities of about 125 W/(m·K) were obtained for the "C775/M350" and "C750/M400" specimens.

Figure 9 . Combined thermal conductivity at different mold temperatures, mean values with n = 3.
Figure 9 . Combined thermal conductivity at different mold temperatures, mean values with n = 3.
Figure 10 . Combined thermal conductivity of pure aluminum and the compound zones, mean values with n = 3.
Figure 10 . Combined thermal conductivity of pure aluminum and the compound zones, mean values with n = 3.

The relationship between thermal conductivity and thickness of the compound zone at 200 °C, which is the maximum applicable temperature for aluminum-copper compounds before phases start growing permanently by diffusion, is summarized in Figure 11 . Lower casting temperatures (left side of Figure 11 ) lead to a smaller thickness of the compound zone and hence to a lower contact resistance, which in turn results in a higher combined thermal conductivity. The error bars mark the scatter of the individual measurements. It is evident that different casting parameters can result in almost identical thicknesses of the compound zones but different thermal conductivities. For example, eight different samples with mold temperatures between 350 and 400 °C and crucible temperatures between 750 and 800 °C all showed similar compound zone thicknesses between 0.73 mm and 0.78 mm (standard deviation of ± 20 µm). Yet, the thermal conductivities of those samples varied from 74 to 132 W/(m·K). Moreover, the standard deviation of the thermal conductivity was larger at lower casting temperatures. This indicates that here the metallurgical bond could no longer be fully established.

Figure 11 . Thermal conductivity in relation to the compound zone thickness; ★: marks different casting parameters resulting in similar compound zone thickness, see main text for details.
Figure 11 . Thermal conductivity in relation to the compound zone thickness; ★: marks different casting parameters resulting in similar compound zone thickness, see main text for details.

The effect of the overall composition ratio of Al to Cu on the thermal conductivity has also been investigated earlier. The data reported by Ho et al. indicates that minimal thermal conductivity (< 50 W/m·K) is reached for copper alloys containing between 70%–95% aluminum. Nevertheless, the influence of the multiphase intermetallic compound on the overall thermal conductivity is difficult to separate from others, since there is currently no way to measure the thermal properties of the individual phases formed in the manufactured compound castings. This issue should be addressed in future work, as findings in this matter could contribute significantly to the further improvement of the casting process. In order to achieve high thermal conductivity, which is of great interest for many highly effective cooling components made of aluminum and copper, a novel compound casting process was developed. Pure aluminum was cast onto a solid pure copper insert in an atmosphere adequate to extreme high vacuum (oxygen-free) to prevent re-oxidation of a de-oxidized copper insert as well as oxidation of the aluminum melt. The results of the present study can be summarized as follows:

Light and electron microscopic investigations of the compounds showed that an oxide-free, metallurgical bond was successfully established between the two materials. In the XHV-adequate atmosphere, aluminum bonds to copper without using coatings or fluxes. Thus, with counteracting the strong tendency of copper to oxidize at elevated temperatures, a major limitation of compound casting, could be overcome by doping monosilane into the inert gas atmosphere. The thermal conductivity measurements showed that similar or even better results compared to those of conventional processes of joining aluminum and copper were achieved. With decreasing casting temperatures ( T crucible and T mold ), the compound zone thickness decreased, and consequently the thermal conductivity increased. Casting parameters of T crucible = 750 °C and T mold = 400 °C as well as T crucible = 775 °C and T mold = 350 °C resulted in the highest thermal conductivity of about 125 W/(m·K). The layers detected using electron microscopy and X-ray diffraction starting from aluminum were: an eutectic structure of copper-rich aluminum solid solutions along with the θ-phase (Al 2 Cu), precipitates from the θ-phase, and finally the η 2 (AlCu) and γ (Al 4 Cu 9 ) intermetallic phases.

Table 2. Suitable Process Temperatures for Formation of Metallurgical Bonds; Process Limit at Lower Temperatures is Marked in Blue

Tool temperature

500 °C

450 °C

400 °C

350 °C

300 °C

Crucible temperature

800 °C

✔

✔

✔

✔

✔

775 °C

✔

✔

✔

✔

X

750 °C

✔

✔

✔

(✔)

X

Fromm, Andreas C., Barienti, Khemais, Selmanovic, Armin, Thürer, Susanne E., Nürnberger, Florian, Maier, Hans Jürgen, Klose, Christian. Oxygen-Free Compound Casting of Aluminum and Copper in a Silane-Doped Inert Gas Atmosphere: A New Approach to Increase Thermal Conductivity. DOI: 10.1007/s40962-022-00910-w. CC BY 4.0。 Original paper · PDF · CC BY 4.0 ·