Inorganic Foundry Binders: Sand Mold Strength, Dimensions, and Casting Surface Quality
Published:
2022-10-08
Different inorganic binders were compared with combinations of silica sand, sintered bauxite, and ceramic sand; ductile iron casting and three-dimensional scanning were used to evaluate mold and casting quality.
Figure 2 . Pattern used for casting trial.
Sand Molding Materials and Casting Experiments
Foundry sodium silicate commonly has a modulus of 2–2.9, the molar ratio of SiO₂ to Na₂O. At equal density, a higher modulus generally increases viscosity. Binder additions are usually 2–4% of sand mass. Hardening can occur chemically with CO₂ or esters, or physically and reversibly through dehydration. Thermal hardening creates a glassy film joining sand grains, but moisture during storage can reduce strength. Initial strength, cycle time, uniform heating and collapsibility remain important constraints. Microwave-hardening trials cited by the paper achieved good mechanical properties with 1.5% binder; lower additions also facilitate reclamation and collapsibility.
The principal type of sand used in the study is silica (SiO 2 > 98%), while some tests were carried out using sintered Bauxite (Al 2 O 3 : 74.2%, Fe 2 O 3 : 15.2%, SiO 2 : 5.7%) and Cerabeads 400 (Short form: CB 400; Al 2 O 3: : 60–62%, SiO 2 : 36–38%). Five different forms of inorganic binders (Binders A to E) were used for the mold study. The content of the sand and binder mixture for each type is given in Table 1 . The values given are used for 1700g of silica sand. Sieve analysis and base permeability test was performed on the sand types used in the study. Organic binders F and G were not used for the mold study but were used for the casting trial to better understand how casting with inorganic binders compares with the organic ones. The reader is referred to for information on mold quality involving organic binders.
For sintered Bauxite and CB 400, the same amount of binder is used. Same volume of sintered Bauxite and CB 400 is used to ensure equal amount of binder per unit volume of sand. It was found in that binder type does not influence mold permeability much. Instead, it is the sand type which influences permeability more. Hence, in this study only base permeability of the sand was measured using Simpson Digital Absolute Permmeter. The mean particle size and specific surface area of the sands were calculated after sieve analysis and bulk density was measured. Grain shape was determined according to test procedure AFS 1107-12-S. Moisture content according to test procedure AFS 2219-00-S. For estimating the specific surface area of the sands, grain shape factors were used from test procedure AFS 1109-12-S, after calculating the theoretical specific surface area using sieve analysis results and equation 4 in (p. 15) and true density values of sands from (Ch. 5) . Strength and loss on ignition (LOI) values were measured from the test bars. For each sand and binder combination, three bending strength test bars were made (measuring 172mm in length and 22.4 mm × 22.4 mm in cross section), and one dog bone specimen was made for tensile strength measurement. For the heat-hardened binders, the strength was measured after heating the test bars to 160 °C for 1 hour. For others that did not require any heat, the bending strength was measured after 24h. This allowed sufficient time for final hardening and ensures a fair comparison. To analyze the thermal and collapsibility behavior of the different binders containing sand molds, residual bending strength was measured at 160 °C, 450 °C, and 900 °C for all binder types. These test bars were heated for 30 minutes before measuring the bending strength. For powder silicates (Binder E), their storage in mixed form with silica sand is also evaluated. This was done by mixing powder silicate and silica sand and storing them for a particular time, some in closed plastic container and some open to air. After the intended storage time, the mixture is taken out, water is added, and test bars were made to measure the strengths. A universal strength tester was used for both bending strength and tensile strength measurements. Only one reading was taken for tensile strength, this was an additional measurement taken with the excess available sample, intended for no statistical purpose but as additional information. Therefore, no error bars are available for the tensile strength measurements.
The loss on ignition values was measured by cutting pieces out of test bars and heating them to 915 °C for 2h. To ensure comparable results between the different types, all the samples were first heated to 160 °C, as two of the binders were heat-hardened at 160 °C. Then the samples were heated to 915 °C in a muffle furnace. Loss on ignition was then measured as the percentage loss in mass before and after heating it to 915 °C. Casting trials were made with 12 different sand and binder combinations. The pattern used was an aluminum metal pattern as shown in Figure 2 . A metal pattern was chosen as some of the molds had to be heated to 160 °C with the pattern inside it. Hence, wooden or most plastic patterns were not compatible in this experiment. One example of the mold made is shown in Figure 3 . 12 such small molds were made for 12 different combinations of sand and binder as shown in Table 2 . These small molds were then combined into a big silica phenolic mold so that the casting could be done at once as shown in Figure 4 . The small molds were stored within plastic packaging before being combined into the large mold. The ambient temperature during the storage was 20–22 °C, and relative humidity between 56% and 64%. The downsprue was in the middle of the runner seen in Figure 4 , and the positions of the mold inserts were documented for later use. Some unintended angling of the inserts can be seen in the molding.
Cast alloy used in the casting trial is a general-purpose ferritic–pearlitic ductile iron, EN GJS 500-7. Metal composition of the alloy is shown in Table 3 . This type of ductile iron was chosen because used pouring temperatures being in a range not requiring refractory coatings, but of high enough thermal exposure to potentially exhibit issues in mold quality. The pouring temperature of the molds is estimated to be in the range 1380 °C–1420 °C, metal temperature having been measured with an immersion lance at 1420 °C before the start of the pouring run. Combined height of downsprue and pouring basin was 250 mm, the mold cavities being in the drag side of the mold. To track each stage of process, 3D scans were taken of the pattern, the molds made and the final castings. The 3D scanner used was based on structured light process, with a claimed accuracy of up to 0.05 mm. From the 3D scans, measurements were made of specific distances and the changes were documented and analyzed in each stage of the process, from pattern to mold and mold to final castings. Mesh-to-mesh comparisons were also made between pattern 3D scan and final castings 3D scan which shows visual deviations between them. Figure 5 shows a scan of the pattern with some marked measurements which were also measured in the mold and casting scans. It was necessary to use an anti-reflective spray to scan the pattern and most of the castings to overcome the limitation of structured light scanning on shiny metal surfaces.
Common methods of assessing as-cast surface conditions include the use of Gar Microfinish comparator C-9 or the SCRATA plate (as per ASTM A802 standard). The operator visually compares castings with these reference plates, therefore offering only discrete assessment levels. It is also very difficult to distinguish between two surfaces which have close surface roughness. In literature, there are also suggestions of using point clouds from 3D scans to analyze surface quality of the whole castings rather than a small representative surface. However, for the purpose of the current study, the use of a 3D optical profilometer was deemed sufficient to evaluate surface quality. For every casting, surface roughness was measured in 3 locations. One on the left flange, one on the right flange and one in the middle. 2mm-by-2mm area was inspected for the measurements. For each location, profile parameters R a and R z values were calculated, and a surface micrograph taken. Regions of pores or sand inclusions were carefully avoided while selecting each 2mm-by-2mm area. It is also possible to calculate surface texture parameters which quantify surfaces from an area viewpoint rather than line profile viewpoint (for example, R a and R z ). The S a parameter is the closest to the R a parameter, although they are fundamentally different. However, if the number of R a values averaged increases, it tends to be closer to the S a parameter, as reported in. The profilometer software(Vision64) provides an R a reading which is an average of roughness of the entire region being measured, hence the R a values reported in this study are also very close approximation of S a parameters.
Since the area of measurement does not lie in a planar surface, a compensation is required. In case of castings, even planar surface by design could deviate due to mold wall displacement and shrinkage differences. In this study, the built-in function of vision 64 software was used for this compensation, which converts any curvature to a planar surface before roughness calculation. Roughness parameters were then noted as reported by the software.
Results for Strength, Dimensions, and Surface Quality
The base properties of the sands used in this study are given in Table 4 , while Figure 6 shows the sieve distribution and sand micrographs are shown in Figure 7 . Density assumptions used for calculation of specific surface area were, silica: 2.65 g/cm 3 , sintered bauxite: 3.3 g/cm 3 and Cerabeads: 2.9 g/cm 3 . Shape assumptions used are shown in Table 4 . CB 400 has almost 3 times the permeability of silica sand due to their large grain size and very uniform circular shape. CB 400 had similar bulk density to silica while sintered Bauxite was much heavier. Sintered Bauxite had a very small negative loss on ignition, which means it gains slight weight due to oxidation. Figure 8 shows the bending strength achieved with the different binder and sand types. Binder A produced the highest bending strength with all types of sand. Specifically, sintered Bauxite and Binder A produced bending strength as high as 448.5 N/cm 2 . For any particular binder type, CB 400 had the least strength. This was anticipated as CB 400 produced low strengths with organic binders as well. Binder E produced intermediary results with all sand types.


Tensile strengths achieved with the different sand and binder types are shown in Figure 9 . Like with bending strength results, the highest tensile strength is achieved with the combination of sintered Bauxite and liquid silicate. All three sands had tensile strength above 50 N/cm 2 . With all sand types, Binder B produced the least strength as was seen with bending strength. Except for Binder E, all other binders produced the highest tensile strength with sintered Bauxite sand. For all inorganic binder types, the loss on ignition was less than what would be expected with organic binders as can be seen in Figure 10 . Powder silicate and sintered Bauxite had the least loss on ignition, while silica and ester-cured liquid silicate (Binder B) had the highest loss on ignition. Except binder D, sintered Bauxite had the lowest loss on ignition. Bending strength and loss on ignition achieved using phenolic and furan binder with different sands could be found in.


Figure 11 shows the residual mold strength of the inorganic molds at different temperatures. All the binders follow a similar profile of residual bending strength with temperature. It gradually decreases at 450 °C and further reduction in 900 °C. No strength could be measured for powder silicate at 900 °C. The heated test bars developed cracks and broke before they could be moved to the tester, as shown in Figure 12 . For Binder B, successive increase in residual strength was noticed after 160 °C. The effect of storing the solid silicate in closed containers is shown in Figure 13 . The bending strength remains above 200 N/cm 2 over the period of 4 weeks while tensile strength remains above 50 N/cm 2 . This confirms that there is not much loss in strength if the powder silicate (Binder E) is kept in mixed form with silica sand up to 4 weeks before use. Storage in open containers was also studied, results shown in Figure 14 .


Bending strength increased after 1 day, and even more after 8 days. All tensile strength values registered were above 60 N/cm 2 . Figures 15 , 16 , and 17 show select castings with visible differences in surface quality. For mesh-to-mesh analysis, the two extremes of the scale used were −1.00 (blue) mm to +1.00 mm (red). The software tracks differences in pattern and casting produced in this range after a best-fit alignment of the separate scans. The blue color corresponds to a place where the casting is smaller than the pattern, and red color to place where the casting is bigger than the pattern and with other gradual changes in color in between as shown in Figure 18 for Sil-F casting. With Sil-F combination contractions could be seen on the outsides of both the flanges. While slight expansion is noticed to areas on both flanges on the inside. This is the expected casting contraction. Rest of the part remained within green to yellow zone. Comparable results were also obtained with Sil-G (silica furan) combination mold. Compared to this, Binder D showed less contraction on the outside. With Binder C, although the outside showed similar contraction, the inside of the flanges showed expansion compared to the pattern, as shown in Figure 19 . With Binder E, there is less contraction on the outside. Stark contrast is obtained with the powder sample as shown in Figure 20 . There is much larger deviation on the inside of both flanges and small contractions can be seen on the top of the top flange. The situation is much improved both in terms of surface roughness and deviations in mesh-to-mesh comparison when a mold release agent was used with Binder E (Combination Sil-EMR).


To track a generalized change in dimensions from pattern to mold and mold to casting, specific distances were measured as shown in Figure 21 . Three different values are taken for P1 across the flange and averaged. Same is done with P2 measurement. Only one value is measured for M1. Tracking the dimensional change was done in two stages: one with only P1 as shown in Table 5 and the other with an average of P2 and M1 as shown in Table 6 . With respect to the inside flange-to-flange distance, a pattern to casting change between −0.89 and −1.11% was seen with all self-setting systems (both inorganic and organic). A high percentage change was seen for Sil-E and Sil-EMR. Sil-A showed a change of −0.9%. The highest was seen with the sintered Bauxite (Bx-A and Bx-E), at slightly more than −2%. For P2 and M1, the pattern to casting change stayed between −0.82 and −1.18% for the self-setting systems. With Sil-A, it was −0.561%, Sil-E at 0.325%, and Sil-EMR −0.34%. Both sintered Bauxite systems had seen positive increase of +0.33% (Bx-A) and +0.16% (Bx-E).
Surface roughness can be visually inspected and compared; differences evident in Figures 15 , 16 , and 17 . Differences can also be seen in 3D scan results of the castings when the differences are relatively large. However, to quantify the surface roughness of R a (arithmetic average of absolute values of profile height deviations from mean line) and R z (average value of absolute values of heights of highest-profile peaks and depths of deepest valleys) were measured. The results are given in Table 7 . Additionally, descriptions of general casting defects observed are noted in the table. Some minor cold shuts were seen in the flange areas of the analyzed castings. These are not listed in the table as those are related to melt flow rather than mold characteristics. Average of 3 R a measurement for each casting is shown in Figure 22 . The pattern in use had an average R a of 4.92µm. The best surface finish was achieved with phenolic binder (Combination Sil-F) at 8.06 µm, followed very closely by the furan binder (Combination Sil-G) at 10.51 µm. Commercially used ester-cured sodium silicate (Sil-C) produced an R a of 12.04 µm and that by geopolymer (Sil-D) 11.95 µm. Very high surface roughness was seen with Sil-E at 55.45 µm. This reduced to 36.91 µm when a mold release agent was used (Sil-EMR). The worst surface roughness was seen with Bx-E (61.9 µm). However, when 50% of silica and 50% of sintered Bauxite was used (Combination Sil-Bx-E), the average surface roughness was 28.12 µm. This was much less than when only either silica or sintered Bauxite was used with Binder E. Some surface micrographs are shown in Figure 23 .

In order to have a better understanding for the high surface roughness value of Sil-E combination, another small test was done. Sil-E mold was made again but this time with a different 3D-printed plastic pattern (thermally resistant up to 200°C). The shape of this pattern was slightly different from the original metal pattern used, but similar in nature. Figure 24 shows the 3D scan of original Sil-E mold, Figure 25 shows the one with 3D-printed pattern. The improvement in surface roughness is quite evident with the new pattern, both visually and also in the 3D scans of the molds. The bending strength achieved in all the different forms of inorganic binders was in acceptable range for foundry use, although the ester-cured sodium silicate was on the lower ranges. However, by altering the amount of binders and/or hardeners the achievable strength can be altered even for specific purposes. As collapsibility is an issue with inorganic binders, residual bending strength was also investigated in this study. All the inorganic binders exhibited a similar trend in residual strength, strength decreasing with increasing temperature but does not fall to zero. Only Binder B showed an increase in residual strength at 450 and 900 °C. Due to binder burnout, organic binders do not retain their strength like inorganic ones do, resulting in their excellent collapsibility. As an example, the tensile strength of furan (1.2%) and silica goes almost zero already at 400 °C. The loss on ignition of inorganic binders with all types of sand was quite small as expected. All organic binders exhibit a much higher loss on ignition as could be seen in. As anticipated, Binder B-system has higher loss on ignition than the fully inorganic binders, the ester-cured sodium silicate being a semi-inorganic system.


Pattern removal was the easiest with the organic systems (Binders F and G). Inorganic binders C and D were also good with pattern release. However, in all the heat-hardened systems pattern removal was challenging. Also, if patterns must be kept inside molds for the whole hardening process, then pattern and mold material can expand or contract at different rates making pattern removal even more challenging. Easy pattern release is also quite important so that minimal damage is made to the mold. The most difficult pattern release was experienced with Binder E in this study. Re-emergence of inorganic binders offers solutions to global sustainability challenges. The challenges are clear to see but there are also significant advantages that foundries can exploit for their benefit. The principal advantage being environmental, while additional benefits like savings in binder purchase, tooling, etc. All the inorganic binders tested here demonstrated good mold strength, maybe even too high in some cases. The loss on ignition values were also very good compared to organic binders. However, the surface finish achieved with organic binders is still superior to inorganic ones, although the commercially available sodium silicate and geopolymers are very close. It is possible to obtain castings through solid sodium silicates, however the surface roughness issues need to be solved before widespread use in foundries is possible. Very encouraging results were obtained with the storage of solid silicates and sand as a mixture. As the manufacturing world is seeking more sustainability and environmental laws getting ever stricter, inorganic binders might become the new norm of foundry use across the globe.
Name | Description | Binder amount | Hardener/co-reactant | Basis for binder/hardener amount selection |
|---|---|---|---|---|
Binder A | Liquid sodium silicate with molar ratio 3.2–3.4. Solid content: 34.1–37.8% | 51 g (3% by mass of sand) | Heated to 160 °C | An intermediate of the usual binder addition rate is chosen |
Binder B | Binder A cured with a mixture of esters | 51 g (3% by mass of sand) | 7.65g (15% by mass of binder) | Ester amounts comparable to commercial binders but tuned to get good output |
Binder C | Ester-cured sodium silicate. Commercially available type for foundry use | 42.5 g (2.5% by mass of sand) | 5.1g (12% by mass of binder) | Manufacturer recommendation |
Binder D | Ester-cured aluminosilicate, more commonly known as geopolymer. Commercially available type for foundry use. Manufacturer claims up to 100% of reclaimed sand could be used | 30.6 g (1.8% by mass of sand) | 4.90g (16% by mass of binder) | Manufacturer recommendation |
Binder E | Hydrated sodium disilicate powder with molar ratio 2.0. Water content: 16-20%. Particle size: 70µm | 14.11g (0.83% by mass of sand) | 19.89g (1.17% by mass of sand) of distilled water is used. Then heated to 160 °C for hardening. | According to19 |
Binder F | Alkaline Phenolic binder. Commercially available type used widely in foundry industry | 25.5g (1.5% by mass of sand) | 6.38g (25% by mass of binder) | Test procedure AFS 3335-04-S27 |
Binder G | Furan. Commercially available type used widely in foundry industry | 17g (1% by mass of sand) | 5.61g (33% by mass of binder) | Manufacturer recommendation |
Left flange | Middle | Right flange | General casting defects observed | ||||
|---|---|---|---|---|---|---|---|
Ra (µm) | Rz (µm) | Ra (µm) | Rz (µm) | Ra (µm) | Rz (µm) | ||
Pattern | 6.66 | 69.30 | 4.22 | 49.32 | 3.90 | 68.69 | |
Sil-A | 16.80 | 136.64 | 28.74 | 194.45 | 13.54 | 105.86 | |
Sil-B | 32.66 | 237.30 | 17.29 | 161.44 | 13.48 | 98.47 | |
Sil-C | 9.23 | 83.94 | 14.51 | 116.27 | 12.38 | 100.49 | |
Sil-D | 17.25 | 197.35 | 7.67 | 88.56 | 10.93 | 87.23 | |
Sil-E | 44.37 | 304.32 | 68.59 | 418.64 | 53.41 | 390.75 | |
Sil-EMR | 49.16 | 281.27 | 14.39 | 142.24 | 47.17 | 318.64 | Minor penetration on left core print |
Sil-F | 10.98 | 80.33 | 7.41 | 58.67 | 5.78 | 46.53 | |
Sil-G | 12.02 | 100.13 | 10.93 | 73.25 | 8.58 | 75.30 | |
Bx-A | 31.74 | 238.48 | 23.26 | 192.93 | 18.63 | 173.61 | Minor penetration on right core print |
Bx-E | 52.85 | 387.30 | 77.33 | 489.18 | 55.52 | 394.92 | Material penetration on left flange |
Sil-Bx-A | 18.34 | 163.34 | 38.01 | 249.20 | 29.58 | 204.15 | |
Sil-Bx-E | 34.99 | 241.08 | 22.98 | 218.62 | 26.40 (Top flange) | 263.75 (Top flange) | Material penetration on right flange |
Anwar, Nurul, Jalava, Kalle, Orkas, Juhani. Experimental Study of Inorganic Foundry Sand Binders for Mold and Cast Quality. DOI: 10.1007/s40962-022-00897-4. CC BY 4.0。 Original paper · PDF · CC BY 4.0 ·
Related News